General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.96 - 8 g/cm³ Show Material materials with Densidad of 7.96 - 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | -196.0 °C | 30 % Show Material materials with Elongación of 30 % | |
-150.0 °C | 35 % Show Material materials with Elongación of 35 % | ||
-80.0 °C | 35 % Show Material materials with Elongación of 35 % | ||
20.0 °C | 40 % Show Material materials with Elongación of 40 % | ||
Elongación A80 transversal | 20.0 °C | 40 % Show Material materials with Elongación A80 transversal of 40 % | |
Elongación transversal | 20.0 °C | 40 % Show Material materials with Elongación transversal of 40 % | |
Límite elástico Rp 0,2 | -196.0 °C | 600 MPa Show Material materials with Límite elástico Rp 0,2 of 600 MPa | |
-150.0 °C | 500 MPa Show Material materials with Límite elástico Rp 0,2 of 500 MPa | ||
-80.0 °C | 380 MPa Show Material materials with Límite elástico Rp 0,2 of 380 MPa | ||
20.0 °C | 280 MPa Show Material materials with Límite elástico Rp 0,2 of 280 MPa | ||
50.0 °C | 254 MPa Show Material materials with Límite elástico Rp 0,2 of 254 MPa | ||
100.0 °C | 211 MPa Show Material materials with Límite elástico Rp 0,2 of 211 MPa | ||
150.0 °C | 185 MPa Show Material materials with Límite elástico Rp 0,2 of 185 MPa | ||
200.0 °C | 167 MPa Show Material materials with Límite elástico Rp 0,2 of 167 MPa | ||
250.0 °C | 155 MPa Show Material materials with Límite elástico Rp 0,2 of 155 MPa | ||
300.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | ||
350.0 °C | 140 MPa Show Material materials with Límite elástico Rp 0,2 of 140 MPa | ||
400.0 °C | 135 MPa Show Material materials with Límite elástico Rp 0,2 of 135 MPa | ||
450.0 °C | 131 MPa Show Material materials with Límite elástico Rp 0,2 of 131 MPa | ||
500.0 °C | 128 MPa Show Material materials with Límite elástico Rp 0,2 of 128 MPa | ||
550.0 °C | 127 MPa Show Material materials with Límite elástico Rp 0,2 of 127 MPa | ||
Límite elástico Rp 1,0 | -196.0 °C | 700 MPa Show Material materials with Límite elástico Rp 1,0 of 700 MPa | |
-150.0 °C | 600 MPa Show Material materials with Límite elástico Rp 1,0 of 600 MPa | ||
-80.0 °C | 450 MPa Show Material materials with Límite elástico Rp 1,0 of 450 MPa | ||
20.0 °C | 320 MPa Show Material materials with Límite elástico Rp 1,0 of 320 MPa | ||
50.0 °C | 292 MPa Show Material materials with Límite elástico Rp 1,0 of 292 MPa | ||
100.0 °C | 246 MPa Show Material materials with Límite elástico Rp 1,0 of 246 MPa | ||
150.0 °C | 218 MPa Show Material materials with Límite elástico Rp 1,0 of 218 MPa | ||
200.0 °C | 198 MPa Show Material materials with Límite elástico Rp 1,0 of 198 MPa | ||
250.0 °C | 183 MPa Show Material materials with Límite elástico Rp 1,0 of 183 MPa | ||
300.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | ||
350.0 °C | 169 MPa Show Material materials with Límite elástico Rp 1,0 of 169 MPa | ||
400.0 °C | 164 MPa Show Material materials with Límite elástico Rp 1,0 of 164 MPa | ||
450.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa | ||
500.0 °C | 158 MPa Show Material materials with Límite elástico Rp 1,0 of 158 MPa | ||
550.0 °C | 157 MPa Show Material materials with Límite elástico Rp 1,0 of 157 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 280 - 300 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 280 - 300 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 320 - 330 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 320 - 330 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | ||
100.0 °C | 190 - 194 GPa Show Material materials with Módulo elástico of 190 - 194 GPa | ||
200.0 °C | 182 - 186 GPa Show Material materials with Módulo elástico of 182 - 186 GPa | ||
300.0 °C | 174 - 179 GPa Show Material materials with Módulo elástico of 174 - 179 GPa | ||
400.0 °C | 166 - 172 GPa Show Material materials with Módulo elástico of 166 - 172 GPa | ||
500.0 °C | 158 - 165 GPa Show Material materials with Módulo elástico of 158 - 165 GPa | ||
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | ||
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | ||
900.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | ||
1000.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | ||
Resistencia a la tracción | -196.0 °C | 1150 MPa Show Material materials with Resistencia a la tracción of 1150 MPa | |
-150.0 °C | 1000 MPa Show Material materials with Resistencia a la tracción of 1000 MPa | ||
-80.0 °C | 800 MPa Show Material materials with Resistencia a la tracción of 800 MPa | ||
20.0 °C | 580 - 780 MPa Show Material materials with Resistencia a la tracción of 580 - 780 MPa | ||
50.0 °C | 557 MPa Show Material materials with Resistencia a la tracción of 557 MPa | ||
100.0 °C | 520 MPa Show Material materials with Resistencia a la tracción of 520 MPa | ||
150.0 °C | 490 MPa Show Material materials with Resistencia a la tracción of 490 MPa | ||
200.0 °C | 460 MPa Show Material materials with Resistencia a la tracción of 460 MPa | ||
250.0 °C | 450 MPa Show Material materials with Resistencia a la tracción of 450 MPa | ||
300.0 °C | 440 MPa Show Material materials with Resistencia a la tracción of 440 MPa | ||
350.0 °C | 435 MPa Show Material materials with Resistencia a la tracción of 435 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 580 - 780 MPa Show Material materials with Resistencia a la tracción transversal of 580 - 780 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 13.3 - 15 W/(m·K) Show Material materials with Conductividad térmica of 13.3 - 15 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Conductividad térmica of 14.9 W/(m·K) | ||
200.0 °C | 16.5 W/(m·K) Show Material materials with Conductividad térmica of 16.5 W/(m·K) | ||
300.0 °C | 18.1 W/(m·K) Show Material materials with Conductividad térmica of 18.1 W/(m·K) | ||
400.0 °C | 19.5 W/(m·K) Show Material materials with Conductividad térmica of 19.5 W/(m·K) | ||
500.0 °C | 21 W/(m·K) Show Material materials with Conductividad térmica of 21 W/(m·K) | ||
600.0 °C | 22.4 W/(m·K) Show Material materials with Conductividad térmica of 22.4 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Conductividad térmica of 23.8 W/(m·K) | ||
800.0 °C | 25.2 W/(m·K) Show Material materials with Conductividad térmica of 25.2 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.5 mm²/s Show Material materials with Difusividad térmica of 3.5 mm²/s | |
100.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
300.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
700.0 °C | 5.1 mm²/s Show Material materials with Difusividad térmica of 5.1 mm²/s | ||
800.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.5E-7 - 7.91E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.5E-7 - 7.91E-7 Ω·m |
100.0 °C | 8.45E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.45E-7 Ω·m | |
200.0 °C | 9.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.19E-7 Ω·m | |
300.0 °C | 9.77E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.77E-7 Ω·m | |
400.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
500.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
600.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
700.0 °C | 1.15E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.15E-6 Ω·m | |
800.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cromo | 16.5 - 18.5 % Show Material materials with Cromo of 16.5 - 18.5 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 2 - 2.5 % Show Material materials with Molibdeno of 2 - 2.5 % |
Nitrógeno | 0.12 - 0.22 % Show Material materials with Nitrógeno of 0.12 - 0.22 % |
Níquel | 10 - 12.5 % Show Material materials with Níquel of 10 - 12.5 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |