General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8 - 8.01 g/cm³ Show Material materials with Densidad of 8 - 8.01 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
Elongación | -196.0 °C | 30 % Show Material materials with Elongación of 30 % |
-150.0 °C | 30 % Show Material materials with Elongación of 30 % | |
-80.0 °C | 30 % Show Material materials with Elongación of 30 % | |
20.0 °C | 35 % Show Material materials with Elongación of 35 % | |
Elongación A80 transversal | 20.0 °C | 35 - 40 % Show Material materials with Elongación A80 transversal of 35 - 40 % |
Elongación transversal | 20.0 °C | 35 - 40 % Show Material materials with Elongación transversal of 35 - 40 % |
Límite elástico Rp 0,2 | -196.0 °C | 600 MPa Show Material materials with Límite elástico Rp 0,2 of 600 MPa |
-150.0 °C | 500 MPa Show Material materials with Límite elástico Rp 0,2 of 500 MPa | |
-80.0 °C | 380 MPa Show Material materials with Límite elástico Rp 0,2 of 380 MPa | |
20.0 °C | 280 MPa Show Material materials with Límite elástico Rp 0,2 of 280 MPa | |
50.0 °C | 254 MPa Show Material materials with Límite elástico Rp 0,2 of 254 MPa | |
100.0 °C | 211 MPa Show Material materials with Límite elástico Rp 0,2 of 211 MPa | |
150.0 °C | 185 MPa Show Material materials with Límite elástico Rp 0,2 of 185 MPa | |
200.0 °C | 167 MPa Show Material materials with Límite elástico Rp 0,2 of 167 MPa | |
250.0 °C | 155 MPa Show Material materials with Límite elástico Rp 0,2 of 155 MPa | |
300.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | |
350.0 °C | 140 MPa Show Material materials with Límite elástico Rp 0,2 of 140 MPa | |
400.0 °C | 135 MPa Show Material materials with Límite elástico Rp 0,2 of 135 MPa | |
450.0 °C | 131 MPa Show Material materials with Límite elástico Rp 0,2 of 131 MPa | |
500.0 °C | 129 MPa Show Material materials with Límite elástico Rp 0,2 of 129 MPa | |
550.0 °C | 127 MPa Show Material materials with Límite elástico Rp 0,2 of 127 MPa | |
Límite elástico Rp 1,0 | -196.0 °C | 700 MPa Show Material materials with Límite elástico Rp 1,0 of 700 MPa |
-150.0 °C | 600 MPa Show Material materials with Límite elástico Rp 1,0 of 600 MPa | |
-80.0 °C | 450 MPa Show Material materials with Límite elástico Rp 1,0 of 450 MPa | |
20.0 °C | 320 MPa Show Material materials with Límite elástico Rp 1,0 of 320 MPa | |
50.0 °C | 292 MPa Show Material materials with Límite elástico Rp 1,0 of 292 MPa | |
100.0 °C | 246 MPa Show Material materials with Límite elástico Rp 1,0 of 246 MPa | |
150.0 °C | 218 MPa Show Material materials with Límite elástico Rp 1,0 of 218 MPa | |
200.0 °C | 198 MPa Show Material materials with Límite elástico Rp 1,0 of 198 MPa | |
250.0 °C | 183 MPa Show Material materials with Límite elástico Rp 1,0 of 183 MPa | |
300.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | |
350.0 °C | 169 MPa Show Material materials with Límite elástico Rp 1,0 of 169 MPa | |
400.0 °C | 164 MPa Show Material materials with Límite elástico Rp 1,0 of 164 MPa | |
450.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa | |
500.0 °C | 158 MPa Show Material materials with Límite elástico Rp 1,0 of 158 MPa | |
550.0 °C | 157 MPa Show Material materials with Límite elástico Rp 1,0 of 157 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 280 - 300 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 280 - 300 MPa |
Límite elástico transversal Rp 1,0 | 20.0 °C | 320 - 330 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 320 - 330 MPa |
Módulo de cizallamiento | 20.0 °C | 77.3 GPa Show Material materials with Módulo de cizallamiento of 77.3 GPa |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | |
100.0 °C | 190 - 194 GPa Show Material materials with Módulo elástico of 190 - 194 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Módulo elástico of 182 - 186 GPa | |
300.0 °C | 174 - 179 GPa Show Material materials with Módulo elástico of 174 - 179 GPa | |
400.0 °C | 166 - 172 GPa Show Material materials with Módulo elástico of 166 - 172 GPa | |
500.0 °C | 158 - 165 GPa Show Material materials with Módulo elástico of 158 - 165 GPa | |
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | |
Resistencia a la tracción | -196.0 °C | 1150 MPa Show Material materials with Resistencia a la tracción of 1150 MPa |
-150.0 °C | 1000 MPa Show Material materials with Resistencia a la tracción of 1000 MPa | |
-80.0 °C | 800 MPa Show Material materials with Resistencia a la tracción of 800 MPa | |
20.0 °C | 580 - 780 MPa Show Material materials with Resistencia a la tracción of 580 - 780 MPa | |
50.0 °C | 557 MPa Show Material materials with Resistencia a la tracción of 557 MPa | |
100.0 °C | 520 MPa Show Material materials with Resistencia a la tracción of 520 MPa | |
150.0 °C | 490 MPa Show Material materials with Resistencia a la tracción of 490 MPa | |
200.0 °C | 460 MPa Show Material materials with Resistencia a la tracción of 460 MPa | |
250.0 °C | 450 MPa Show Material materials with Resistencia a la tracción of 450 MPa | |
300.0 °C | 440 MPa Show Material materials with Resistencia a la tracción of 440 MPa | |
350.0 °C | 435 MPa Show Material materials with Resistencia a la tracción of 435 MPa | |
400.0 °C | 435 MPa Show Material materials with Resistencia a la tracción of 435 MPa | |
500.0 °C | 430 MPa Show Material materials with Resistencia a la tracción of 430 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 580 - 780 MPa Show Material materials with Resistencia a la tracción transversal of 580 - 780 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 13.5 - 15 W/(m·K) Show Material materials with Conductividad térmica of 13.5 - 15 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Conductividad térmica of 14.9 W/(m·K) | ||
200.0 °C | 16.7 W/(m·K) Show Material materials with Conductividad térmica of 16.7 W/(m·K) | ||
300.0 °C | 18.3 W/(m·K) Show Material materials with Conductividad térmica of 18.3 W/(m·K) | ||
400.0 °C | 19.8 W/(m·K) Show Material materials with Conductividad térmica of 19.8 W/(m·K) | ||
500.0 °C | 21.3 W/(m·K) Show Material materials with Conductividad térmica of 21.3 W/(m·K) | ||
600.0 °C | 22.7 W/(m·K) Show Material materials with Conductividad térmica of 22.7 W/(m·K) | ||
700.0 °C | 24.2 W/(m·K) Show Material materials with Conductividad térmica of 24.2 W/(m·K) | ||
800.0 °C | 25.6 W/(m·K) Show Material materials with Conductividad térmica of 25.6 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.6 mm²/s Show Material materials with Difusividad térmica of 3.6 mm²/s | |
100.0 °C | 3.7 mm²/s Show Material materials with Difusividad térmica of 3.7 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
300.0 °C | 4.4 mm²/s Show Material materials with Difusividad térmica of 4.4 mm²/s | ||
400.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
600.0 °C | 4.9 mm²/s Show Material materials with Difusividad térmica of 4.9 mm²/s | ||
700.0 °C | 5.2 mm²/s Show Material materials with Difusividad térmica of 5.2 mm²/s | ||
800.0 °C | 5.5 mm²/s Show Material materials with Difusividad térmica of 5.5 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | -270 - 0 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -270 - 0 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.5E-7 - 7.75E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.5E-7 - 7.75E-7 Ω·m |
100.0 °C | 8.42E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.42E-7 Ω·m | |
200.0 °C | 9.04E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.04E-7 Ω·m | |
300.0 °C | 9.62E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.62E-7 Ω·m | |
400.0 °C | 1.01E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.01E-6 Ω·m | |
500.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
600.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
700.0 °C | 1.13E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.13E-6 Ω·m | |
800.0 °C | 1.16E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.16E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cromo | 16.5 - 18.5 % Show Material materials with Cromo of 16.5 - 18.5 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 2.5 - 3 % Show Material materials with Molibdeno of 2.5 - 3 % |
Nitrógeno | 0.12 - 0.22 % Show Material materials with Nitrógeno of 0.12 - 0.22 % |
Níquel | 11 - 14 % Show Material materials with Níquel of 11 - 14 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |