General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8 - 8.08 g/cm³ Show Material materials with Densidad of 8 - 8.08 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación A80 transversal | 20.0 °C | 40 % Show Material materials with Elongación A80 transversal of 40 % | |
Elongación transversal | 20.0 °C | 40 % Show Material materials with Elongación transversal of 40 % | |
Límite elástico Rp 0,2 | 50.0 °C | 209 MPa Show Material materials with Límite elástico Rp 0,2 of 209 MPa | |
100.0 °C | 190 MPa Show Material materials with Límite elástico Rp 0,2 of 190 MPa | ||
150.0 °C | 175 MPa Show Material materials with Límite elástico Rp 0,2 of 175 MPa | ||
200.0 °C | 160 MPa Show Material materials with Límite elástico Rp 0,2 of 160 MPa | ||
250.0 °C | 155 MPa Show Material materials with Límite elástico Rp 0,2 of 155 MPa | ||
300.0 °C | 150 MPa Show Material materials with Límite elástico Rp 0,2 of 150 MPa | ||
350.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | ||
400.0 °C | 135 MPa Show Material materials with Límite elástico Rp 0,2 of 135 MPa | ||
450.0 °C | 125 MPa Show Material materials with Límite elástico Rp 0,2 of 125 MPa | ||
500.0 °C | 120 MPa Show Material materials with Límite elástico Rp 0,2 of 120 MPa | ||
550.0 °C | 115 MPa Show Material materials with Límite elástico Rp 0,2 of 115 MPa | ||
Límite elástico Rp 1,0 | 50.0 °C | 245 MPa Show Material materials with Límite elástico Rp 1,0 of 245 MPa | |
100.0 °C | 220 MPa Show Material materials with Límite elástico Rp 1,0 of 220 MPa | ||
150.0 °C | 205 MPa Show Material materials with Límite elástico Rp 1,0 of 205 MPa | ||
200.0 °C | 190 MPa Show Material materials with Límite elástico Rp 1,0 of 190 MPa | ||
250.0 °C | 185 MPa Show Material materials with Límite elástico Rp 1,0 of 185 MPa | ||
300.0 °C | 180 MPa Show Material materials with Límite elástico Rp 1,0 of 180 MPa | ||
350.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | ||
400.0 °C | 165 MPa Show Material materials with Límite elástico Rp 1,0 of 165 MPa | ||
450.0 °C | 155 MPa Show Material materials with Límite elástico Rp 1,0 of 155 MPa | ||
500.0 °C | 150 MPa Show Material materials with Límite elástico Rp 1,0 of 150 MPa | ||
550.0 °C | 145 MPa Show Material materials with Límite elástico Rp 1,0 of 145 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 220 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 220 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 260 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 260 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 20.0 °C | 191 - 195 GPa Show Material materials with Módulo elástico of 191 - 195 GPa | |
100.0 °C | 186 - 190 GPa Show Material materials with Módulo elástico of 186 - 190 GPa | ||
200.0 °C | 179 - 182 GPa Show Material materials with Módulo elástico of 179 - 182 GPa | ||
300.0 °C | 172 - 174 GPa Show Material materials with Módulo elástico of 172 - 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Módulo elástico of 166 GPa | ||
500.0 °C | 158 - 159 GPa Show Material materials with Módulo elástico of 158 - 159 GPa | ||
Resistencia a la tracción | 20.0 °C | 500 - 700 MPa Show Material materials with Resistencia a la tracción of 500 - 700 MPa | |
50.0 °C | 485 MPa Show Material materials with Resistencia a la tracción of 485 MPa | ||
100.0 °C | 460 MPa Show Material materials with Resistencia a la tracción of 460 MPa | ||
150.0 °C | 445 MPa Show Material materials with Resistencia a la tracción of 445 MPa | ||
200.0 °C | 430 MPa Show Material materials with Resistencia a la tracción of 430 MPa | ||
250.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
300.0 °C | 400 MPa Show Material materials with Resistencia a la tracción of 400 MPa | ||
350.0 °C | 395 MPa Show Material materials with Resistencia a la tracción of 395 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 500 - 700 MPa Show Material materials with Resistencia a la tracción transversal of 500 - 700 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 450 - 452 J/(kg·K) Show Material materials with Calor específico of 450 - 452 J/(kg·K) | |
100.0 °C | 463 J/(kg·K) Show Material materials with Calor específico of 463 J/(kg·K) | ||
200.0 °C | 474 J/(kg·K) Show Material materials with Calor específico of 474 J/(kg·K) | ||
300.0 °C | 483 J/(kg·K) Show Material materials with Calor específico of 483 J/(kg·K) | ||
400.0 °C | 491 J/(kg·K) Show Material materials with Calor específico of 491 J/(kg·K) | ||
500.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100.0 °C | 1.51E-5 - 1.58E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.51E-5 - 1.58E-5 1/K | |
200.0 °C | 1.55E-5 - 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.55E-5 - 1.61E-5 1/K | ||
300.0 °C | 1.58E-5 - 1.65E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.58E-5 - 1.65E-5 1/K | ||
400.0 °C | 1.62E-5 - 1.69E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.62E-5 - 1.69E-5 1/K | ||
500.0 °C | 1.66E-5 - 1.73E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.66E-5 - 1.73E-5 1/K | ||
Conductividad térmica | 20.0 °C | 11.7 - 12 W/(m·K) Show Material materials with Conductividad térmica of 11.7 - 12 W/(m·K) | |
100.0 °C | 13.2 W/(m·K) Show Material materials with Conductividad térmica of 13.2 W/(m·K) | ||
200.0 °C | 15 W/(m·K) Show Material materials with Conductividad térmica of 15 W/(m·K) | ||
300.0 °C | 16.8 W/(m·K) Show Material materials with Conductividad térmica of 16.8 W/(m·K) | ||
400.0 °C | 18.5 W/(m·K) Show Material materials with Conductividad térmica of 18.5 W/(m·K) | ||
500.0 °C | 20.2 W/(m·K) Show Material materials with Conductividad térmica of 20.2 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.2 mm²/s Show Material materials with Difusividad térmica of 3.2 mm²/s | |
100.0 °C | 3.5 mm²/s Show Material materials with Difusividad térmica of 3.5 mm²/s | ||
200.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | ||
300.0 °C | 4.1 mm²/s Show Material materials with Difusividad térmica of 4.1 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1E-6 - 1.04E-6 Ω·m Show Material materials with Resistividad eléctrica of 1E-6 - 1.04E-6 Ω·m |
100.0 °C | 1.07E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.07E-6 Ω·m | |
200.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
300.0 °C | 1.13E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.13E-6 Ω·m | |
400.0 °C | 1.16E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.16E-6 Ω·m | |
500.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % |
Carbono | 0.02 % Show Material materials with Carbono of 0.02 % |
Cobre | 0.7 - 1.5 % Show Material materials with Cobre of 0.7 - 1.5 % |
Cromo | 26 - 28 % Show Material materials with Cromo of 26 - 28 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 3 - 4 % Show Material materials with Molibdeno of 3 - 4 % |
Nitrógeno | 0.1 - 0.11 % Show Material materials with Nitrógeno of 0.1 - 0.11 % |
Níquel | 30 - 32 % Show Material materials with Níquel of 30 - 32 % |
Silicona | 0.7 % Show Material materials with Silicona of 0.7 % |