General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.65 - 7.7 g/cm³ Show Material materials with Densidad of 7.65 - 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Ferritic Stainless Steel |
Dureza Brinell | 20.0 °C | 192 [-] Show Material materials with Dureza Brinell of 192 [-] | |
Elongación | 20.0 °C | 20 % Show Material materials with Elongación of 20 % | |
Elongación transversal | 20.0 °C | 15 % Show Material materials with Elongación transversal of 15 % | |
Límite elástico Rp 0,2 | 20.0 °C | 220 MPa Show Material materials with Límite elástico Rp 0,2 of 220 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 220 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 220 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Ferritic Stainless Steel |
Módulo elástico | 20.0 °C | 218 GPa Show Material materials with Módulo elástico of 218 GPa | |
100.0 °C | 213 GPa Show Material materials with Módulo elástico of 213 GPa | ||
200.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | ||
300.0 °C | 198 GPa Show Material materials with Módulo elástico of 198 GPa | ||
400.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | ||
500.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | ||
600.0 °C | 167 GPa Show Material materials with Módulo elástico of 167 GPa | ||
Resistencia a la tracción | 20.0 °C | 420 - 620 MPa Show Material materials with Resistencia a la tracción of 420 - 620 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 420 - 620 MPa Show Material materials with Resistencia a la tracción transversal of 420 - 620 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 425 - 450 J/(kg·K) Show Material materials with Calor específico of 425 - 450 J/(kg·K) | |
100.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
200.0 °C | 489 J/(kg·K) Show Material materials with Calor específico of 489 J/(kg·K) | ||
300.0 °C | 508 J/(kg·K) Show Material materials with Calor específico of 508 J/(kg·K) | ||
400.0 °C | 527 J/(kg·K) Show Material materials with Calor específico of 527 J/(kg·K) | ||
500.0 °C | 550 J/(kg·K) Show Material materials with Calor específico of 550 J/(kg·K) | ||
600.0 °C | 579 J/(kg·K) Show Material materials with Calor específico of 579 J/(kg·K) | ||
700.0 °C | 618 J/(kg·K) Show Material materials with Calor específico of 618 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 1/K | |
20.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | ||
100.0 °C | 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.13E-5 1/K | ||
200.0 °C | 1.15E-5 - 1.18E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 - 1.18E-5 1/K | ||
300.0 °C | 1.23E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.23E-5 1/K | ||
400.0 °C | 1.2E-5 - 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 - 1.27E-5 1/K | ||
500.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
600.0 °C | 1.25E-5 - 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 - 1.32E-5 1/K | ||
800.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
Conductividad térmica | 20.0 °C | 20.5 - 23 W/(m·K) Show Material materials with Conductividad térmica of 20.5 - 23 W/(m·K) | |
100.0 °C | 21.9 W/(m·K) Show Material materials with Conductividad térmica of 21.9 W/(m·K) | ||
200.0 °C | 23.2 W/(m·K) Show Material materials with Conductividad térmica of 23.2 W/(m·K) | ||
300.0 °C | 24.2 W/(m·K) Show Material materials with Conductividad térmica of 24.2 W/(m·K) | ||
400.0 °C | 24.9 W/(m·K) Show Material materials with Conductividad térmica of 24.9 W/(m·K) | ||
500.0 °C | 25 - 25.4 W/(m·K) Show Material materials with Conductividad térmica of 25 - 25.4 W/(m·K) | ||
600.0 °C | 25.6 W/(m·K) Show Material materials with Conductividad térmica of 25.6 W/(m·K) | ||
700.0 °C | 25.5 W/(m·K) Show Material materials with Conductividad térmica of 25.5 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 6.3 mm²/s Show Material materials with Difusividad térmica of 6.3 mm²/s | |
100.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
200.0 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | ||
300.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
400.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
500.0 °C | 5 mm²/s Show Material materials with Difusividad térmica of 5 mm²/s | ||
600.0 °C | 4.4 mm²/s Show Material materials with Difusividad térmica of 4.4 mm²/s | ||
700.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | ||
Temperatura de fusión | 1425 - 1530 °C Show Material materials with Temperatura de fusión of 1425 - 1530 °C | Typical for Ferritic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 700 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 700 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7E-7 - 7.07E-7 Ω·m Show Material materials with Resistividad eléctrica of 7E-7 - 7.07E-7 Ω·m |
100.0 °C | 7.43E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.43E-7 Ω·m | |
200.0 °C | 7.94E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.94E-7 Ω·m | |
300.0 °C | 8.52E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.52E-7 Ω·m | |
400.0 °C | 9.16E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.16E-7 Ω·m | |
500.0 °C | 9.87E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.87E-7 Ω·m | |
600.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
700.0 °C | 1.15E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.15E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.5 - 1 % Show Material materials with Aluminio of 0.5 - 1 % |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.12 % Show Material materials with Carbono of 0.12 % |
Cromo | 6 - 8 % Show Material materials with Cromo of 6 - 8 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Silicona | 0.5 - 1 % Show Material materials with Silicona of 0.5 - 1 % |