General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.4 g/cm³ Show Material materials with Densidad of 8.4 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 200 [-] Show Material materials with Dureza Brinell of 200 [-] |
Elongación | 20.0 °C | 30 % Show Material materials with Elongación of 30 % |
Elongación A80 | 20.0 °C | 30 % Show Material materials with Elongación A80 of 30 % |
Límite elástico Rp 0,2 | 20.0 °C | 240 MPa Show Material materials with Límite elástico Rp 0,2 of 240 MPa |
Módulo elástico | 20.0 °C | 214 GPa Show Material materials with Módulo elástico of 214 GPa |
100.0 °C | 209 GPa Show Material materials with Módulo elástico of 209 GPa | |
200.0 °C | 205 GPa Show Material materials with Módulo elástico of 205 GPa | |
300.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | |
400.0 °C | 194 GPa Show Material materials with Módulo elástico of 194 GPa | |
500.0 °C | 187 GPa Show Material materials with Módulo elástico of 187 GPa | |
600.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | |
700.0 °C | 172 GPa Show Material materials with Módulo elástico of 172 GPa | |
800.0 °C | 163 GPa Show Material materials with Módulo elástico of 163 GPa | |
900.0 °C | 153 GPa Show Material materials with Módulo elástico of 153 GPa | |
1000.0 °C | 143 GPa Show Material materials with Módulo elástico of 143 GPa | |
Resistencia a la tracción | 20.0 °C | 500 - 850 MPa Show Material materials with Resistencia a la tracción of 500 - 850 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 455 - 460 J/(kg·K) Show Material materials with Calor específico of 455 - 460 J/(kg·K) | |
100.0 °C | 475 J/(kg·K) Show Material materials with Calor específico of 475 J/(kg·K) | ||
200.0 °C | 495 J/(kg·K) Show Material materials with Calor específico of 495 J/(kg·K) | ||
300.0 °C | 508 J/(kg·K) Show Material materials with Calor específico of 508 J/(kg·K) | ||
400.0 °C | 525 J/(kg·K) Show Material materials with Calor específico of 525 J/(kg·K) | ||
500.0 °C | 550 J/(kg·K) Show Material materials with Calor específico of 550 J/(kg·K) | ||
600.0 °C | 572 J/(kg·K) Show Material materials with Calor específico of 572 J/(kg·K) | ||
700.0 °C | 602 J/(kg·K) Show Material materials with Calor específico of 602 J/(kg·K) | ||
800.0 °C | 620 J/(kg·K) Show Material materials with Calor específico of 620 J/(kg·K) | ||
900.0 °C | 630 J/(kg·K) Show Material materials with Calor específico of 630 J/(kg·K) | ||
1000.0 °C | 635 J/(kg·K) Show Material materials with Calor específico of 635 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100.0 °C | 1.37E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.37E-5 1/K | |
200.0 °C | 1.39E-5 - 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.39E-5 - 1.41E-5 1/K | ||
300.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | ||
400.0 °C | 1.45E-5 - 1.48E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 - 1.48E-5 1/K | ||
500.0 °C | 1.51E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.51E-5 1/K | ||
600.0 °C | 1.53E-5 - 1.54E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.53E-5 - 1.54E-5 1/K | ||
700.0 °C | 1.58E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.58E-5 1/K | ||
800.0 °C | 1.61E-5 - 1.62E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 - 1.62E-5 1/K | ||
900.0 °C | 1.64E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.64E-5 1/K | ||
1000.0 °C | 1.68E-5 - 1.69E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.68E-5 - 1.69E-5 1/K | ||
Conductividad térmica | 20.0 °C | 14.8 - 15 W/(m·K) Show Material materials with Conductividad térmica of 14.8 - 15 W/(m·K) | |
100.0 °C | 15.8 W/(m·K) Show Material materials with Conductividad térmica of 15.8 W/(m·K) | ||
200.0 °C | 17 W/(m·K) Show Material materials with Conductividad térmica of 17 W/(m·K) | ||
300.0 °C | 18.4 W/(m·K) Show Material materials with Conductividad térmica of 18.4 W/(m·K) | ||
400.0 °C | 20 W/(m·K) Show Material materials with Conductividad térmica of 20 W/(m·K) | ||
500.0 °C | 22 W/(m·K) Show Material materials with Conductividad térmica of 22 W/(m·K) | ||
600.0 °C | 24 W/(m·K) Show Material materials with Conductividad térmica of 24 W/(m·K) | ||
700.0 °C | 25.7 W/(m·K) Show Material materials with Conductividad térmica of 25.7 W/(m·K) | ||
800.0 °C | 27.5 W/(m·K) Show Material materials with Conductividad térmica of 27.5 W/(m·K) | ||
900.0 °C | 29.4 W/(m·K) Show Material materials with Conductividad térmica of 29.4 W/(m·K) | ||
1000.0 °C | 31.2 W/(m·K) Show Material materials with Conductividad térmica of 31.2 W/(m·K) | ||
Temperatura de fusión | 1200 - 1480 °C Show Material materials with Temperatura de fusión of 1200 - 1480 °C | Typical for Nickel Chromium Iron Alloy | |
Temperatura máx. de funcionamiento, largo | 0 - 1150 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 1150 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m |
100.0 °C | 1.04E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.04E-6 Ω·m | |
200.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
300.0 °C | 1.07E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.07E-6 Ω·m | |
400.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
500.0 °C | 1.11E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.11E-6 Ω·m | |
600.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
700.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
800.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
900.0 °C | 1.13E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.13E-6 Ω·m | |
1000.0 °C | 1.14E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.14E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.3 % Show Material materials with Aluminio of 0.3 % |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.05 - 0.1 % Show Material materials with Carbono of 0.05 - 0.1 % |
Cobre | 0.5 % Show Material materials with Cobre of 0.5 % |
Cromo | 14 - 17 % Show Material materials with Cromo of 14 - 17 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Hierro | 6 - 10 % Show Material materials with Hierro of 6 - 10 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Níquel | 72 % Show Material materials with Níquel of 72 % |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % |
Titanio | 0.3 % Show Material materials with Titanio of 0.3 % |