General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.4 g/cm³ Show Material materials with Densidad of 8.4 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 240 [-] Show Material materials with Dureza Brinell of 240 [-] |
Elongación | 20.0 °C | 25 - 30 % Show Material materials with Elongación of 25 - 30 % |
Elongación A80 | 20.0 °C | 30 % Show Material materials with Elongación A80 of 30 % |
Límite elástico Rp 0,2 | 20.0 °C | 345 - 415 MPa Show Material materials with Límite elástico Rp 0,2 of 345 - 415 MPa |
Módulo elástico | 20.0 °C | 209 GPa Show Material materials with Módulo elástico of 209 GPa |
100.0 °C | 202 GPa Show Material materials with Módulo elástico of 202 GPa | |
200.0 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa | |
300.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | |
400.0 °C | 185 GPa Show Material materials with Módulo elástico of 185 GPa | |
500.0 °C | 178 GPa Show Material materials with Módulo elástico of 178 GPa | |
600.0 °C | 170 GPa Show Material materials with Módulo elástico of 170 GPa | |
700.0 °C | 162 GPa Show Material materials with Módulo elástico of 162 GPa | |
800.0 °C | 153 GPa Show Material materials with Módulo elástico of 153 GPa | |
900.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
1000.0 °C | 128 GPa Show Material materials with Módulo elástico of 128 GPa | |
Resistencia a la tracción | 20.0 °C | 760 - 1050 MPa Show Material materials with Resistencia a la tracción of 760 - 1050 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 20.0 °C | 410 - 415 J/(kg·K) Show Material materials with Calor específico of 410 - 415 J/(kg·K) |
100.0 °C | 435 J/(kg·K) Show Material materials with Calor específico of 435 J/(kg·K) | |
200.0 °C | 460 J/(kg·K) Show Material materials with Calor específico of 460 J/(kg·K) | |
300.0 °C | 480 J/(kg·K) Show Material materials with Calor específico of 480 J/(kg·K) | |
400.0 °C | 505 J/(kg·K) Show Material materials with Calor específico of 505 J/(kg·K) | |
500.0 °C | 525 J/(kg·K) Show Material materials with Calor específico of 525 J/(kg·K) | |
600.0 °C | 550 J/(kg·K) Show Material materials with Calor específico of 550 J/(kg·K) | |
700.0 °C | 575 J/(kg·K) Show Material materials with Calor específico of 575 J/(kg·K) | |
800.0 °C | 600 J/(kg·K) Show Material materials with Calor específico of 600 J/(kg·K) | |
900.0 °C | 625 J/(kg·K) Show Material materials with Calor específico of 625 J/(kg·K) | |
1000.0 °C | 650 J/(kg·K) Show Material materials with Calor específico of 650 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.28E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.28E-5 1/K |
200.0 °C | 1.11E-5 - 1.31E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.11E-5 - 1.31E-5 1/K | |
300.0 °C | 1.34E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34E-5 1/K | |
400.0 °C | 1.26E-5 - 1.37E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.26E-5 - 1.37E-5 1/K | |
500.0 °C | 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41E-5 1/K | |
600.0 °C | 1.38E-5 - 1.46E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.38E-5 - 1.46E-5 1/K | |
700.0 °C | 1.52E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.52E-5 1/K | |
800.0 °C | 1.49E-5 - 1.58E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 - 1.58E-5 1/K | |
900.0 °C | 1.64E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.64E-5 1/K | |
1000.0 °C | 1.58E-5 - 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.58E-5 - 1.7E-5 1/K | |
Conductividad térmica | 20.0 °C | 9.8 - 10 W/(m·K) Show Material materials with Conductividad térmica of 9.8 - 10 W/(m·K) |
100.0 °C | 11.2 W/(m·K) Show Material materials with Conductividad térmica of 11.2 W/(m·K) | |
200.0 °C | 12.8 W/(m·K) Show Material materials with Conductividad térmica of 12.8 W/(m·K) | |
300.0 °C | 14.4 W/(m·K) Show Material materials with Conductividad térmica of 14.4 W/(m·K) | |
400.0 °C | 16.3 W/(m·K) Show Material materials with Conductividad térmica of 16.3 W/(m·K) | |
500.0 °C | 17 - 17.3 W/(m·K) Show Material materials with Conductividad térmica of 17 - 17.3 W/(m·K) | |
600.0 °C | 19.3 W/(m·K) Show Material materials with Conductividad térmica of 19.3 W/(m·K) | |
700.0 °C | 21 W/(m·K) Show Material materials with Conductividad térmica of 21 W/(m·K) | |
800.0 °C | 22.6 W/(m·K) Show Material materials with Conductividad térmica of 22.6 W/(m·K) | |
900.0 °C | 24.6 W/(m·K) Show Material materials with Conductividad térmica of 24.6 W/(m·K) | |
1000.0 °C | 26.7 W/(m·K) Show Material materials with Conductividad térmica of 26.7 W/(m·K) | |
Temperatura máx. de funcionamiento, largo | 0 - 1000 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 1000 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.28E-6 - 1.29E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.28E-6 - 1.29E-6 Ω·m |
100.0 °C | 1.3E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.3E-6 Ω·m | |
200.0 °C | 1.32E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.32E-6 Ω·m | |
300.0 °C | 1.33E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.33E-6 Ω·m | |
400.0 °C | 1.35E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.35E-6 Ω·m | |
500.0 °C | 1.36E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.36E-6 Ω·m | |
600.0 °C | 1.36E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.36E-6 Ω·m | |
700.0 °C | 1.36E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.36E-6 Ω·m | |
800.0 °C | 1.36E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.36E-6 Ω·m | |
900.0 °C | 1.35E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.35E-6 Ω·m | |
1000.0 °C | 1.32E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.32E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.4 % Show Material materials with Aluminio of 0.4 % |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.03 - 0.1 % Show Material materials with Carbono of 0.03 - 0.1 % |
Cobalto | 1 % Show Material materials with Cobalto of 1 % |
Cobre | 0.5 % Show Material materials with Cobre of 0.5 % |
Cromo | 20 - 23 % Show Material materials with Cromo of 20 - 23 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Hierro | 5 % Show Material materials with Hierro of 5 % |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % |
Molibdeno | 8 - 10 % Show Material materials with Molibdeno of 8 - 10 % |
Níquel | 58 % Show Material materials with Níquel of 58 % |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % |
Titanio | 0.4 % Show Material materials with Titanio of 0.4 % |