General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.7 g/cm³ Show Material materials with Densidad of 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Martensitic Stainless Steel |
Elongación | 20.0 °C | 15 % Show Material materials with Elongación of 15 % | |
Límite elástico Rp 0,2 | 20.0 °C | 540 MPa Show Material materials with Límite elástico Rp 0,2 of 540 MPa | |
200.0 °C | 450 MPa Show Material materials with Límite elástico Rp 0,2 of 450 MPa | ||
300.0 °C | 430 MPa Show Material materials with Límite elástico Rp 0,2 of 430 MPa | ||
350.0 °C | 410 MPa Show Material materials with Límite elástico Rp 0,2 of 410 MPa | ||
400.0 °C | 390 MPa Show Material materials with Límite elástico Rp 0,2 of 390 MPa | ||
450.0 °C | 370 MPa Show Material materials with Límite elástico Rp 0,2 of 370 MPa | ||
500.0 °C | 340 MPa Show Material materials with Límite elástico Rp 0,2 of 340 MPa | ||
550.0 °C | 290 MPa Show Material materials with Límite elástico Rp 0,2 of 290 MPa | ||
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Martensitic Stainless Steel |
Módulo elástico | 20.0 °C | 216 GPa Show Material materials with Módulo elástico of 216 GPa | |
100.0 °C | 209 GPa Show Material materials with Módulo elástico of 209 GPa | ||
200.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | ||
300.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | ||
400.0 °C | 179 GPa Show Material materials with Módulo elástico of 179 GPa | ||
500.0 °C | 167 GPa Show Material materials with Módulo elástico of 167 GPa | ||
600.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | ||
Resistencia a la tracción | 20.0 °C | 740 - 880 MPa Show Material materials with Resistencia a la tracción of 740 - 880 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 460 J/(kg·K) Show Material materials with Calor específico of 460 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
200.0 °C | 1.1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 1/K | ||
300.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | ||
400.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
500.0 °C | 1.22E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 1/K | ||
600.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | ||
Conductividad térmica | 20.0 °C | 24 W/(m·K) Show Material materials with Conductividad térmica of 24 W/(m·K) | |
300.0 °C | 25 W/(m·K) Show Material materials with Conductividad térmica of 25 W/(m·K) | ||
400.0 °C | 26 W/(m·K) Show Material materials with Conductividad térmica of 26 W/(m·K) | ||
500.0 °C | 27 W/(m·K) Show Material materials with Conductividad térmica of 27 W/(m·K) | ||
600.0 °C | 27 W/(m·K) Show Material materials with Conductividad térmica of 27 W/(m·K) | ||
Temperatura de fusión | 1370 - 1530 °C Show Material materials with Temperatura de fusión of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 300 - 610 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 300 - 610 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 4.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % |
Carbono | 0.2 - 0.26 % Show Material materials with Carbono of 0.2 - 0.26 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 11.3 - 12.2 % Show Material materials with Cromo of 11.3 - 12.2 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.5 - 0.8 % Show Material materials with Manganeso of 0.5 - 0.8 % |
Molibdeno | 1 - 1.2 % Show Material materials with Molibdeno of 1 - 1.2 % |
Níquel | 1 % Show Material materials with Níquel of 1 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |
Vanadio | 0.25 - 0.35 % Show Material materials with Vanadio of 0.25 - 0.35 % |
Wolframio | 0.5 % Show Material materials with Wolframio of 0.5 % |