General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.7 g/cm³ Show Material materials with Densidad of 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Martensitic Stainless Steel |
Elongación | 20.0 °C | 15 % Show Material materials with Elongación of 15 % | |
Límite elástico Rp 0,2 | 20.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | |
100.0 °C | 515 MPa Show Material materials with Límite elástico Rp 0,2 of 515 MPa | ||
200.0 °C | 485 MPa Show Material materials with Límite elástico Rp 0,2 of 485 MPa | ||
300.0 °C | 455 MPa Show Material materials with Límite elástico Rp 0,2 of 455 MPa | ||
350.0 °C | 440 MPa Show Material materials with Límite elástico Rp 0,2 of 440 MPa | ||
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Martensitic Stainless Steel |
Módulo elástico | 23.0 °C | 220 GPa Show Material materials with Módulo elástico of 220 GPa | Typical for Martensitic Stainless Steel |
Resistencia a la tracción | 20.0 °C | 760 - 960 MPa Show Material materials with Resistencia a la tracción of 760 - 960 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 460 J/(kg·K) Show Material materials with Calor específico of 460 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
300.0 °C | 1.1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 1/K | ||
500.0 °C | 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 1/K | ||
Conductividad térmica | 50.0 °C | 26 W/(m·K) Show Material materials with Conductividad térmica of 26 W/(m·K) | |
100.0 °C | 27 W/(m·K) Show Material materials with Conductividad térmica of 27 W/(m·K) | ||
Temperatura de fusión | 1370 - 1530 °C Show Material materials with Temperatura de fusión of 1370 - 1530 °C | Typical for Martensitic Stainless Steel |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Resistividad eléctrica | 23.0 °C | 6E-7 Ω·m Show Material materials with Resistividad eléctrica of 6E-7 Ω·m | Typical for Martensitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Carbono | 0.06 % Show Material materials with Carbono of 0.06 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 12 - 13.5 % Show Material materials with Cromo of 12 - 13.5 % |
Estaño | 0.03 % Show Material materials with Estaño of 0.03 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Molibdeno | 0.7 % Show Material materials with Molibdeno of 0.7 % |
Níquel | 3.5 - 5 % Show Material materials with Níquel of 3.5 - 5 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |
Vanadio | 0.08 % Show Material materials with Vanadio of 0.08 % |