General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Elongación | 20.0 °C | 16 % Show Material materials with Elongación of 16 % | |
Elongación transversal | 20.0 °C | 14 % Show Material materials with Elongación transversal of 14 % | |
Límite elástico Rp 0,2 | 20.0 °C | 590 MPa Show Material materials with Límite elástico Rp 0,2 of 590 MPa | |
150.0 °C | 575 MPa Show Material materials with Límite elástico Rp 0,2 of 575 MPa | ||
200.0 °C | 570 MPa Show Material materials with Límite elástico Rp 0,2 of 570 MPa | ||
250.0 °C | 560 MPa Show Material materials with Límite elástico Rp 0,2 of 560 MPa | ||
300.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | ||
350.0 °C | 510 MPa Show Material materials with Límite elástico Rp 0,2 of 510 MPa | ||
400.0 °C | 470 MPa Show Material materials with Límite elástico Rp 0,2 of 470 MPa | ||
450.0 °C | 420 MPa Show Material materials with Límite elástico Rp 0,2 of 420 MPa | ||
500.0 °C | 370 MPa Show Material materials with Límite elástico Rp 0,2 of 370 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 590 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 590 MPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Resistencia a la tracción | 20.0 °C | 740 - 880 MPa Show Material materials with Resistencia a la tracción of 740 - 880 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 740 - 880 MPa Show Material materials with Resistencia a la tracción transversal of 740 - 880 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | ||
Conductividad térmica | 20.0 °C | 25.7 W/(m·K) Show Material materials with Conductividad térmica of 25.7 W/(m·K) | |
100.0 °C | 27.4 W/(m·K) Show Material materials with Conductividad térmica of 27.4 W/(m·K) | ||
200.0 °C | 28.5 W/(m·K) Show Material materials with Conductividad térmica of 28.5 W/(m·K) | ||
300.0 °C | 28.9 W/(m·K) Show Material materials with Conductividad térmica of 28.9 W/(m·K) | ||
400.0 °C | 28.5 W/(m·K) Show Material materials with Conductividad térmica of 28.5 W/(m·K) | ||
500.0 °C | 27.7 W/(m·K) Show Material materials with Conductividad térmica of 27.7 W/(m·K) | ||
600.0 °C | 26.8 W/(m·K) Show Material materials with Conductividad térmica of 26.8 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | |
100.0 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | ||
200.0 °C | 6.9 mm²/s Show Material materials with Difusividad térmica of 6.9 mm²/s | ||
300.0 °C | 6.6 mm²/s Show Material materials with Difusividad térmica of 6.6 mm²/s | ||
400.0 °C | 6.1 mm²/s Show Material materials with Difusividad térmica of 6.1 mm²/s | ||
500.0 °C | 5.3 mm²/s Show Material materials with Difusividad térmica of 5.3 mm²/s | ||
600.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Temperatura máx. de funcionamiento, largo | 200 - 550 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 200 - 550 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 4.05E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.05E-7 Ω·m |
100.0 °C | 4.67E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.67E-7 Ω·m | |
200.0 °C | 5.53E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.53E-7 Ω·m | |
300.0 °C | 6.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.5E-7 Ω·m | |
400.0 °C | 7.62E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.62E-7 Ω·m | |
500.0 °C | 8.92E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.92E-7 Ω·m | |
600.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.04 % Show Material materials with Aluminio of 0.04 % |
Azufre | 0.01 - 0.02 % Show Material materials with Azufre of 0.01 - 0.02 % |
Carbono | 0.17 - 0.23 % Show Material materials with Carbono of 0.17 - 0.23 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 3 - 3.3 % Show Material materials with Cromo of 3 - 3.3 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.3 - 0.5 % Show Material materials with Manganeso of 0.3 - 0.5 % |
Molibdeno | 0.5 - 0.6 % Show Material materials with Molibdeno of 0.5 - 0.6 % |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % |
Silicona | 0.15 - 0.35 % Show Material materials with Silicona of 0.15 - 0.35 % |
Vanadio | 0.45 - 0.55 % Show Material materials with Vanadio of 0.45 - 0.55 % |