General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.77 g/cm³ Show Material materials with Densidad of 7.77 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Elongación | 20.0 °C | 20 % Show Material materials with Elongación of 20 % | |
Elongación transversal | 20.0 °C | 18 % Show Material materials with Elongación transversal of 18 % | |
Límite elástico Rp 0,2 | 20.0 °C | 210 MPa Show Material materials with Límite elástico Rp 0,2 of 210 MPa | |
100.0 °C | 187 MPa Show Material materials with Límite elástico Rp 0,2 of 187 MPa | ||
150.0 °C | 186 MPa Show Material materials with Límite elástico Rp 0,2 of 186 MPa | ||
200.0 °C | 178 MPa Show Material materials with Límite elástico Rp 0,2 of 178 MPa | ||
250.0 °C | 177 MPa Show Material materials with Límite elástico Rp 0,2 of 177 MPa | ||
300.0 °C | 175 MPa Show Material materials with Límite elástico Rp 0,2 of 175 MPa | ||
350.0 °C | 171 MPa Show Material materials with Límite elástico Rp 0,2 of 171 MPa | ||
400.0 °C | 164 MPa Show Material materials with Límite elástico Rp 0,2 of 164 MPa | ||
450.0 °C | 153 MPa Show Material materials with Límite elástico Rp 0,2 of 153 MPa | ||
500.0 °C | 142 MPa Show Material materials with Límite elástico Rp 0,2 of 142 MPa | ||
550.0 °C | 120 MPa Show Material materials with Límite elástico Rp 0,2 of 120 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 210 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 210 MPa | |
Módulo elástico | 20.0 °C | 218 GPa Show Material materials with Módulo elástico of 218 GPa | |
100.0 °C | 213 GPa Show Material materials with Módulo elástico of 213 GPa | ||
200.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | ||
300.0 °C | 198 GPa Show Material materials with Módulo elástico of 198 GPa | ||
400.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | ||
500.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | ||
600.0 °C | 167 GPa Show Material materials with Módulo elástico of 167 GPa | ||
700.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
Resistencia a la tracción | 20.0 °C | 460 - 640 MPa Show Material materials with Resistencia a la tracción of 460 - 640 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 460 - 640 MPa Show Material materials with Resistencia a la tracción transversal of 460 - 640 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 429 J/(kg·K) Show Material materials with Calor específico of 429 J/(kg·K) | |
100.0 °C | 464 J/(kg·K) Show Material materials with Calor específico of 464 J/(kg·K) | ||
200.0 °C | 492 J/(kg·K) Show Material materials with Calor específico of 492 J/(kg·K) | ||
300.0 °C | 511 J/(kg·K) Show Material materials with Calor específico of 511 J/(kg·K) | ||
400.0 °C | 531 J/(kg·K) Show Material materials with Calor específico of 531 J/(kg·K) | ||
500.0 °C | 554 J/(kg·K) Show Material materials with Calor específico of 554 J/(kg·K) | ||
600.0 °C | 585 J/(kg·K) Show Material materials with Calor específico of 585 J/(kg·K) | ||
700.0 °C | 626 J/(kg·K) Show Material materials with Calor específico of 626 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 1/K | |
20.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | ||
100.0 °C | 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.13E-5 1/K | ||
200.0 °C | 1.18E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.18E-5 1/K | ||
300.0 °C | 1.23E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.23E-5 1/K | ||
400.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
500.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
600.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
700.0 °C | 1.33E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.33E-5 1/K | ||
Conductividad térmica | 20.0 °C | 20.7 W/(m·K) Show Material materials with Conductividad térmica of 20.7 W/(m·K) | |
100.0 °C | 22.6 W/(m·K) Show Material materials with Conductividad térmica of 22.6 W/(m·K) | ||
200.0 °C | 24.4 W/(m·K) Show Material materials with Conductividad térmica of 24.4 W/(m·K) | ||
300.0 °C | 25.8 W/(m·K) Show Material materials with Conductividad térmica of 25.8 W/(m·K) | ||
400.0 °C | 26.9 W/(m·K) Show Material materials with Conductividad térmica of 26.9 W/(m·K) | ||
500.0 °C | 27.8 W/(m·K) Show Material materials with Conductividad térmica of 27.8 W/(m·K) | ||
600.0 °C | 28.5 W/(m·K) Show Material materials with Conductividad térmica of 28.5 W/(m·K) | ||
700.0 °C | 28.8 W/(m·K) Show Material materials with Conductividad térmica of 28.8 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 6.2 mm²/s Show Material materials with Difusividad térmica of 6.2 mm²/s | |
100.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
200.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
300.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
400.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
500.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
700.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 550 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 550 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 5.03E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.03E-7 Ω·m |
100.0 °C | 5.67E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.67E-7 Ω·m | |
200.0 °C | 6.47E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.47E-7 Ω·m | |
300.0 °C | 7.27E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.27E-7 Ω·m | |
400.0 °C | 8.09E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.09E-7 Ω·m | |
500.0 °C | 8.9E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.9E-7 Ω·m | |
600.0 °C | 9.72E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.72E-7 Ω·m | |
700.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.04 % Show Material materials with Aluminio of 0.04 % |
Azufre | 0.01 - 0.02 % Show Material materials with Azufre of 0.01 - 0.02 % |
Carbono | 0.08 - 0.15 % Show Material materials with Carbono of 0.08 - 0.15 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 8 - 10 % Show Material materials with Cromo of 8 - 10 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.3 - 0.6 % Show Material materials with Manganeso of 0.3 - 0.6 % |
Molibdeno | 0.9 - 1.1 % Show Material materials with Molibdeno of 0.9 - 1.1 % |
Silicona | 0.25 - 1 % Show Material materials with Silicona of 0.25 - 1 % |