General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8 g/cm³ Show Material materials with Densidad of 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | 20.0 °C | 35 % Show Material materials with Elongación of 35 % | |
Elongación transversal | 20.0 °C | 30 % Show Material materials with Elongación transversal of 30 % | |
Límite elástico Rp 0,2 | 20.0 °C | 220 MPa Show Material materials with Límite elástico Rp 0,2 of 220 MPa | |
50.0 °C | 213 MPa Show Material materials with Límite elástico Rp 0,2 of 213 MPa | ||
100.0 °C | 188 MPa Show Material materials with Límite elástico Rp 0,2 of 188 MPa | ||
150.0 °C | 171 MPa Show Material materials with Límite elástico Rp 0,2 of 171 MPa | ||
200.0 °C | 161 MPa Show Material materials with Límite elástico Rp 0,2 of 161 MPa | ||
250.0 °C | 153 MPa Show Material materials with Límite elástico Rp 0,2 of 153 MPa | ||
300.0 °C | 148 MPa Show Material materials with Límite elástico Rp 0,2 of 148 MPa | ||
350.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | ||
400.0 °C | 144 MPa Show Material materials with Límite elástico Rp 0,2 of 144 MPa | ||
450.0 °C | 141 MPa Show Material materials with Límite elástico Rp 0,2 of 141 MPa | ||
500.0 °C | 139 MPa Show Material materials with Límite elástico Rp 0,2 of 139 MPa | ||
550.0 °C | 136 MPa Show Material materials with Límite elástico Rp 0,2 of 136 MPa | ||
Límite elástico Rp 1,0 | 20.0 °C | 270 MPa Show Material materials with Límite elástico Rp 1,0 of 270 MPa | |
50.0 °C | 254 MPa Show Material materials with Límite elástico Rp 1,0 of 254 MPa | ||
100.0 °C | 232 MPa Show Material materials with Límite elástico Rp 1,0 of 232 MPa | ||
150.0 °C | 210 MPa Show Material materials with Límite elástico Rp 1,0 of 210 MPa | ||
200.0 °C | 195 MPa Show Material materials with Límite elástico Rp 1,0 of 195 MPa | ||
250.0 °C | 190 MPa Show Material materials with Límite elástico Rp 1,0 of 190 MPa | ||
300.0 °C | 187 MPa Show Material materials with Límite elástico Rp 1,0 of 187 MPa | ||
350.0 °C | 184 MPa Show Material materials with Límite elástico Rp 1,0 of 184 MPa | ||
400.0 °C | 182 MPa Show Material materials with Límite elástico Rp 1,0 of 182 MPa | ||
450.0 °C | 179 MPa Show Material materials with Límite elástico Rp 1,0 of 179 MPa | ||
500.0 °C | 178 MPa Show Material materials with Límite elástico Rp 1,0 of 178 MPa | ||
550.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 220 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 220 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 270 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 270 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 20.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | |
100.0 °C | 201 GPa Show Material materials with Módulo elástico of 201 GPa | ||
200.0 °C | 193 GPa Show Material materials with Módulo elástico of 193 GPa | ||
300.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | ||
400.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
500.0 °C | 165 GPa Show Material materials with Módulo elástico of 165 GPa | ||
600.0 °C | 158 GPa Show Material materials with Módulo elástico of 158 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 480 J/(kg·K) Show Material materials with Calor específico of 480 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.57E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.57E-5 1/K | |
200.0 °C | 1.68E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.68E-5 1/K | ||
300.0 °C | 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.77E-5 1/K | ||
400.0 °C | 1.83E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.83E-5 1/K | ||
500.0 °C | 1.86E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.86E-5 1/K | ||
600.0 °C | 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9E-5 1/K | ||
Conductividad térmica | 20.0 °C | 12.5 W/(m·K) Show Material materials with Conductividad térmica of 12.5 W/(m·K) | |
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.4E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.4E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Boro | 3E-3 - 9E-3 % Show Material materials with Boro of 3E-3 - 9E-3 % |
Carbono | 0.06 - 0.15 % Show Material materials with Carbono of 0.06 - 0.15 % |
Cromo | 14 - 16 % Show Material materials with Cromo of 14 - 16 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 5.5 - 7 % Show Material materials with Manganeso of 5.5 - 7 % |
Molibdeno | 0.8 - 1.2 % Show Material materials with Molibdeno of 0.8 - 1.2 % |
Niobio | 0.75 - 1.25 % Show Material materials with Niobio of 0.75 - 1.25 % |
Nitrógeno | 0.06 - 0.14 % Show Material materials with Nitrógeno of 0.06 - 0.14 % |
Níquel | 9 - 11 % Show Material materials with Níquel of 9 - 11 % |
Silicona | 0.2 - 1 % Show Material materials with Silicona of 0.2 - 1 % |
Vanadio | 0.15 - 0.4 % Show Material materials with Vanadio of 0.15 - 0.4 % |