General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel |
Elongación | 20.0 °C | 22 % Show Material materials with Elongación of 22 % | |
Límite elástico | 20.0 °C | 315 - 355 MPa Show Material materials with Límite elástico of 315 - 355 MPa | |
Límite elástico Rp 0,2 | 50.0 °C | 280 - 340 MPa Show Material materials with Límite elástico Rp 0,2 of 280 - 340 MPa | |
100.0 °C | 250 - 310 MPa Show Material materials with Límite elástico Rp 0,2 of 250 - 310 MPa | ||
150.0 °C | 225 - 285 MPa Show Material materials with Límite elástico Rp 0,2 of 225 - 285 MPa | ||
200.0 °C | 200 - 260 MPa Show Material materials with Límite elástico Rp 0,2 of 200 - 260 MPa | ||
250.0 °C | 175 - 235 MPa Show Material materials with Límite elástico Rp 0,2 of 175 - 235 MPa | ||
300.0 °C | 155 - 215 MPa Show Material materials with Límite elástico Rp 0,2 of 155 - 215 MPa | ||
Módulo elástico | 23.0 °C | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel |
Resistencia a la tracción | 20.0 °C | 450 - 630 MPa Show Material materials with Resistencia a la tracción of 450 - 630 MPa |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.018 % Show Material materials with Aluminio of 0.018 % |
Azufre | 0.01 - 0.015 % Show Material materials with Azufre of 0.01 - 0.015 % |
Boro | 5E-3 % Show Material materials with Boro of 5E-3 % |
Carbono | 0.16 % Show Material materials with Carbono of 0.16 % |
Circonio | 0.05 % Show Material materials with Circonio of 0.05 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 1.5 % Show Material materials with Manganeso of 1.5 % |
Molibdeno | 0.25 % Show Material materials with Molibdeno of 0.25 % |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % |
Nitrógeno | 0.02 % Show Material materials with Nitrógeno of 0.02 % |
Níquel | 0.5 % Show Material materials with Níquel of 0.5 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % |
Vanadio | 0.06 % Show Material materials with Vanadio of 0.06 % |