General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.85 - 7.86 g/cm³ Show Material materials with Densidad of 7.85 - 7.86 g/cm³ |
50.0 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | |
100.0 °C | 7.82 g/cm³ Show Material materials with Densidad of 7.82 g/cm³ | |
150.0 °C | 7.81 g/cm³ Show Material materials with Densidad of 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ Show Material materials with Densidad of 7.79 g/cm³ | |
250.0 °C | 7.77 g/cm³ Show Material materials with Densidad of 7.77 g/cm³ | |
300.0 °C | 7.76 g/cm³ Show Material materials with Densidad of 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ Show Material materials with Densidad of 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ Show Material materials with Densidad of 7.72 g/cm³ | |
450.0 °C | 7.7 g/cm³ Show Material materials with Densidad of 7.7 g/cm³ | |
500.0 °C | 7.68 g/cm³ Show Material materials with Densidad of 7.68 g/cm³ | |
550.0 °C | 7.66 g/cm³ Show Material materials with Densidad of 7.66 g/cm³ | |
600.0 °C | 7.64 g/cm³ Show Material materials with Densidad of 7.64 g/cm³ | |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] |
50.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
100.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
150.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
250.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
300.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
350.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
450.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
500.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
550.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
600.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
Elongación | 20.0 °C | 19 - 24 % Show Material materials with Elongación of 19 - 24 % |
Límite elástico | 20.0 °C | 220 - 275 MPa Show Material materials with Límite elástico of 220 - 275 MPa |
Límite elástico Rp 0,2 | 50.0 °C | 218 - 273 MPa Show Material materials with Límite elástico Rp 0,2 of 218 - 273 MPa |
100.0 °C | 211 - 264 MPa Show Material materials with Límite elástico Rp 0,2 of 211 - 264 MPa | |
150.0 °C | 200 - 250 MPa Show Material materials with Límite elástico Rp 0,2 of 200 - 250 MPa | |
200.0 °C | 186 - 233 MPa Show Material materials with Límite elástico Rp 0,2 of 186 - 233 MPa | |
250.0 °C | 171 - 213 MPa Show Material materials with Límite elástico Rp 0,2 of 171 - 213 MPa | |
300.0 °C | 155 - 194 MPa Show Material materials with Límite elástico Rp 0,2 of 155 - 194 MPa | |
350.0 °C | 140 - 175 MPa Show Material materials with Límite elástico Rp 0,2 of 140 - 175 MPa | |
400.0 °C | 127 - 159 MPa Show Material materials with Límite elástico Rp 0,2 of 127 - 159 MPa | |
450.0 °C | 118 - 147 MPa Show Material materials with Límite elástico Rp 0,2 of 118 - 147 MPa | |
500.0 °C | 113 - 141 MPa Show Material materials with Límite elástico Rp 0,2 of 113 - 141 MPa | |
Módulo de cizallamiento | 20.0 °C | 82.6 GPa Show Material materials with Módulo de cizallamiento of 82.6 GPa |
50.0 °C | 82.21 GPa Show Material materials with Módulo de cizallamiento of 82.21 GPa | |
100.0 °C | 81.23 GPa Show Material materials with Módulo de cizallamiento of 81.23 GPa | |
150.0 °C | 79.95 GPa Show Material materials with Módulo de cizallamiento of 79.95 GPa | |
200.0 °C | 78.48 GPa Show Material materials with Módulo de cizallamiento of 78.48 GPa | |
250.0 °C | 76.81 GPa Show Material materials with Módulo de cizallamiento of 76.81 GPa | |
300.0 °C | 75.05 GPa Show Material materials with Módulo de cizallamiento of 75.05 GPa | |
350.0 °C | 73.38 GPa Show Material materials with Módulo de cizallamiento of 73.38 GPa | |
400.0 °C | 71.61 GPa Show Material materials with Módulo de cizallamiento of 71.61 GPa | |
450.0 °C | 69.75 GPa Show Material materials with Módulo de cizallamiento of 69.75 GPa | |
500.0 °C | 67.98 GPa Show Material materials with Módulo de cizallamiento of 67.98 GPa | |
550.0 °C | 66.22 GPa Show Material materials with Módulo de cizallamiento of 66.22 GPa | |
600.0 °C | 64.35 GPa Show Material materials with Módulo de cizallamiento of 64.35 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa |
20.0 °C | 212 - 212.48 GPa Show Material materials with Módulo elástico of 212 - 212.48 GPa | |
50.0 °C | 211.6 GPa Show Material materials with Módulo elástico of 211.6 GPa | |
100.0 °C | 207 - 209.25 GPa Show Material materials with Módulo elástico of 207 - 209.25 GPa | |
150.0 °C | 206.11 GPa Show Material materials with Módulo elástico of 206.11 GPa | |
200.0 °C | 199 - 202.48 GPa Show Material materials with Módulo elástico of 199 - 202.48 GPa | |
250.0 °C | 198.36 GPa Show Material materials with Módulo elástico of 198.36 GPa | |
300.0 °C | 192 - 194.14 GPa Show Material materials with Módulo elástico of 192 - 194.14 GPa | |
350.0 °C | 189.82 GPa Show Material materials with Módulo elástico of 189.82 GPa | |
400.0 °C | 184 - 185.51 GPa Show Material materials with Módulo elástico of 184 - 185.51 GPa | |
450.0 °C | 180.99 GPa Show Material materials with Módulo elástico of 180.99 GPa | |
500.0 °C | 175 - 176.48 GPa Show Material materials with Módulo elástico of 175 - 176.48 GPa | |
550.0 °C | 171.97 GPa Show Material materials with Módulo elástico of 171.97 GPa | |
600.0 °C | 164 - 166.97 GPa Show Material materials with Módulo elástico of 164 - 166.97 GPa | |
Resistencia a la tracción | 20.0 °C | 420 - 590 MPa Show Material materials with Resistencia a la tracción of 420 - 590 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | ||
Conductividad térmica | 20.0 °C | 52.1 W/(m·K) Show Material materials with Conductividad térmica of 52.1 W/(m·K) | |
100.0 °C | 51.2 W/(m·K) Show Material materials with Conductividad térmica of 51.2 W/(m·K) | ||
200.0 °C | 48.7 W/(m·K) Show Material materials with Conductividad térmica of 48.7 W/(m·K) | ||
300.0 °C | 45.5 W/(m·K) Show Material materials with Conductividad térmica of 45.5 W/(m·K) | ||
400.0 °C | 42.3 W/(m·K) Show Material materials with Conductividad térmica of 42.3 W/(m·K) | ||
500.0 °C | 39.1 W/(m·K) Show Material materials with Conductividad térmica of 39.1 W/(m·K) | ||
600.0 °C | 36 W/(m·K) Show Material materials with Conductividad térmica of 36 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 14.4 mm²/s Show Material materials with Difusividad térmica of 14.4 mm²/s | |
100.0 °C | 13.2 mm²/s Show Material materials with Difusividad térmica of 13.2 mm²/s | ||
200.0 °C | 11.7 mm²/s Show Material materials with Difusividad térmica of 11.7 mm²/s | ||
300.0 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | ||
400.0 °C | 9 mm²/s Show Material materials with Difusividad térmica of 9 mm²/s | ||
500.0 °C | 7.5 mm²/s Show Material materials with Difusividad térmica of 7.5 mm²/s | ||
600.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Molybdenum Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 530 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 530 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 2E-7 - 2.16E-7 Ω·m Show Material materials with Resistividad eléctrica of 2E-7 - 2.16E-7 Ω·m |
50.0 °C | 2.37E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.37E-7 Ω·m | |
100.0 °C | 2.5E-7 - 2.68E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.5E-7 - 2.68E-7 Ω·m | |
150.0 °C | 3.02E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.02E-7 Ω·m | |
200.0 °C | 3.24E-7 - 3.39E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.24E-7 - 3.39E-7 Ω·m | |
250.0 °C | 3.8E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.8E-7 Ω·m | |
300.0 °C | 4.12E-7 - 4.25E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.12E-7 - 4.25E-7 Ω·m | |
350.0 °C | 4.74E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.74E-7 Ω·m | |
400.0 °C | 5.14E-7 - 5.27E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.14E-7 - 5.27E-7 Ω·m | |
450.0 °C | 5.83E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.83E-7 Ω·m | |
500.0 °C | 6.33E-7 - 6.42E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.33E-7 - 6.42E-7 Ω·m | |
550.0 °C | 7.08E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.08E-7 Ω·m | |
600.0 °C | 7.69E-7 - 7.78E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.69E-7 - 7.78E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.01 - 0.025 % Show Material materials with Azufre of 0.01 - 0.025 % |
Carbono | 0.12 - 0.2 % Show Material materials with Carbono of 0.12 - 0.2 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.4 - 0.9 % Show Material materials with Manganeso of 0.4 - 0.9 % |
Molibdeno | 0.25 - 0.35 % Show Material materials with Molibdeno of 0.25 - 0.35 % |
Nitrógeno | 0.01 % Show Material materials with Nitrógeno of 0.01 % |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % |