General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | Typical for Chromium Molybdenum Steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Elongación | 20.0 °C | 15 % Show Material materials with Elongación of 15 % | |
Estricción | 20.0 °C | 50 % Show Material materials with Estricción of 50 % | |
Límite elástico Rp 0,2 | 20.0 °C | 660 MPa Show Material materials with Límite elástico Rp 0,2 of 660 MPa | |
50.0 °C | 642 MPa Show Material materials with Límite elástico Rp 0,2 of 642 MPa | ||
100.0 °C | 624 MPa Show Material materials with Límite elástico Rp 0,2 of 624 MPa | ||
150.0 °C | 603 MPa Show Material materials with Límite elástico Rp 0,2 of 603 MPa | ||
200.0 °C | 595 MPa Show Material materials with Límite elástico Rp 0,2 of 595 MPa | ||
250.0 °C | 581 MPa Show Material materials with Límite elástico Rp 0,2 of 581 MPa | ||
300.0 °C | 573 MPa Show Material materials with Límite elástico Rp 0,2 of 573 MPa | ||
350.0 °C | 559 MPa Show Material materials with Límite elástico Rp 0,2 of 559 MPa | ||
400.0 °C | 537 MPa Show Material materials with Límite elástico Rp 0,2 of 537 MPa | ||
450.0 °C | 508 MPa Show Material materials with Límite elástico Rp 0,2 of 508 MPa | ||
500.0 °C | 464 MPa Show Material materials with Límite elástico Rp 0,2 of 464 MPa | ||
550.0 °C | 406 MPa Show Material materials with Límite elástico Rp 0,2 of 406 MPa | ||
600.0 °C | 334 MPa Show Material materials with Límite elástico Rp 0,2 of 334 MPa | ||
Módulo elástico | 23.0 °C | 200 - 215 GPa Show Material materials with Módulo elástico of 200 - 215 GPa | Typical for Chromium Molybdenum Steel |
Resistencia a la tracción | 20.0 °C | 820 - 1000 MPa Show Material materials with Resistencia a la tracción of 820 - 1000 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 448 - 502 J/(kg·K) Show Material materials with Calor específico of 448 - 502 J/(kg·K) | Typical for Chromium Molybdenum Steel |
Coeficiente de dilatación térmica | 23.0 °C | 1.1E-5 - 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.4E-5 1/K | Typical for Chromium Molybdenum Steel |
Conductividad térmica | 23.0 °C | 36 - 43 W/(m·K) Show Material materials with Conductividad térmica of 36 - 43 W/(m·K) | Typical for Chromium Molybdenum Steel |
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.015 - 0.08 % Show Material materials with Aluminio of 0.015 - 0.08 % |
Arsénico | 0.02 % Show Material materials with Arsénico of 0.02 % |
Azufre | 0.015 - 0.02 % Show Material materials with Azufre of 0.015 - 0.02 % |
Boro | 0.001 - 0.01 % Show Material materials with Boro of 0.001 - 0.01 % |
Carbono | 0.17 - 0.23 % Show Material materials with Carbono of 0.17 - 0.23 % |
Cobre | 0.2 % Show Material materials with Cobre of 0.2 % |
Cromo | 0.9 - 1.2 % Show Material materials with Cromo of 0.9 - 1.2 % |
Estaño | 0.02 % Show Material materials with Estaño of 0.02 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Manganeso | 0.35 - 0.75 % Show Material materials with Manganeso of 0.35 - 0.75 % |
Molibdeno | 0.9 - 1.1 % Show Material materials with Molibdeno of 0.9 - 1.1 % |
Níquel | 0.2 % Show Material materials with Níquel of 0.2 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |
Titanio | 0.07 - 0.15 % Show Material materials with Titanio of 0.07 - 0.15 % |
Vanadio | 0.6 - 0.8 % Show Material materials with Vanadio of 0.6 - 0.8 % |