General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 g/cm³ Show Material materials with Densidad of 7.9 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Ferritic Stainless Steel |
Elongación | -196.0 °C | 35 % Show Material materials with Elongación of 35 % | |
-150.0 °C | 35 % Show Material materials with Elongación of 35 % | ||
-80.0 °C | 40 % Show Material materials with Elongación of 40 % | ||
20.0 °C | 40 % Show Material materials with Elongación of 40 % | ||
Elongación A80 transversal | 20.0 °C | 40 % Show Material materials with Elongación A80 transversal of 40 % | |
Elongación transversal | 20.0 °C | 40 % Show Material materials with Elongación transversal of 40 % | |
Límite elástico Rp 0,2 | -196.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | |
-150.0 °C | 450 MPa Show Material materials with Límite elástico Rp 0,2 of 450 MPa | ||
-80.0 °C | 385 MPa Show Material materials with Límite elástico Rp 0,2 of 385 MPa | ||
20.0 °C | 270 MPa Show Material materials with Límite elástico Rp 0,2 of 270 MPa | ||
50.0 °C | 246 MPa Show Material materials with Límite elástico Rp 0,2 of 246 MPa | ||
100.0 °C | 205 MPa Show Material materials with Límite elástico Rp 0,2 of 205 MPa | ||
150.0 °C | 175 MPa Show Material materials with Límite elástico Rp 0,2 of 175 MPa | ||
200.0 °C | 157 MPa Show Material materials with Límite elástico Rp 0,2 of 157 MPa | ||
250.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | ||
300.0 °C | 136 MPa Show Material materials with Límite elástico Rp 0,2 of 136 MPa | ||
350.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | ||
400.0 °C | 125 MPa Show Material materials with Límite elástico Rp 0,2 of 125 MPa | ||
450.0 °C | 121 MPa Show Material materials with Límite elástico Rp 0,2 of 121 MPa | ||
500.0 °C | 119 MPa Show Material materials with Límite elástico Rp 0,2 of 119 MPa | ||
550.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | ||
Límite elástico Rp 1,0 | -196.0 °C | 650 MPa Show Material materials with Límite elástico Rp 1,0 of 650 MPa | |
-150.0 °C | 550 MPa Show Material materials with Límite elástico Rp 1,0 of 550 MPa | ||
-80.0 °C | 455 MPa Show Material materials with Límite elástico Rp 1,0 of 455 MPa | ||
20.0 °C | 310 MPa Show Material materials with Límite elástico Rp 1,0 of 310 MPa | ||
50.0 °C | 284 MPa Show Material materials with Límite elástico Rp 1,0 of 284 MPa | ||
100.0 °C | 240 MPa Show Material materials with Límite elástico Rp 1,0 of 240 MPa | ||
150.0 °C | 210 MPa Show Material materials with Límite elástico Rp 1,0 of 210 MPa | ||
200.0 °C | 187 MPa Show Material materials with Límite elástico Rp 1,0 of 187 MPa | ||
250.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | ||
300.0 °C | 167 MPa Show Material materials with Límite elástico Rp 1,0 of 167 MPa | ||
350.0 °C | 161 MPa Show Material materials with Límite elástico Rp 1,0 of 161 MPa | ||
400.0 °C | 156 MPa Show Material materials with Límite elástico Rp 1,0 of 156 MPa | ||
450.0 °C | 152 MPa Show Material materials with Límite elástico Rp 1,0 of 152 MPa | ||
500.0 °C | 149 MPa Show Material materials with Límite elástico Rp 1,0 of 149 MPa | ||
550.0 °C | 147 MPa Show Material materials with Límite elástico Rp 1,0 of 147 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 270 - 290 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 270 - 290 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 310 - 320 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 310 - 320 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Ferritic Stainless Steel |
Módulo elástico | 20.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | |
100.0 °C | 194 - 195 GPa Show Material materials with Módulo elástico of 194 - 195 GPa | ||
200.0 °C | 185 - 186 GPa Show Material materials with Módulo elástico of 185 - 186 GPa | ||
300.0 °C | 179 - 180 GPa Show Material materials with Módulo elástico of 179 - 180 GPa | ||
400.0 °C | 172 GPa Show Material materials with Módulo elástico of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Módulo elástico of 165 GPa | ||
Resistencia a la tracción | -196.0 °C | 1350 MPa Show Material materials with Resistencia a la tracción of 1350 MPa | |
-150.0 °C | 1180 MPa Show Material materials with Resistencia a la tracción of 1180 MPa | ||
-80.0 °C | 890 MPa Show Material materials with Resistencia a la tracción of 890 MPa | ||
20.0 °C | 550 - 750 MPa Show Material materials with Resistencia a la tracción of 550 - 750 MPa | ||
50.0 °C | 527 MPa Show Material materials with Resistencia a la tracción of 527 MPa | ||
100.0 °C | 490 MPa Show Material materials with Resistencia a la tracción of 490 MPa | ||
150.0 °C | 460 MPa Show Material materials with Resistencia a la tracción of 460 MPa | ||
200.0 °C | 430 MPa Show Material materials with Resistencia a la tracción of 430 MPa | ||
250.0 °C | 420 MPa Show Material materials with Resistencia a la tracción of 420 MPa | ||
300.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
350.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 550 - 750 MPa Show Material materials with Resistencia a la tracción transversal of 550 - 750 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.6E-5 - 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.7E-5 1/K | |
200.0 °C | 1.65E-5 - 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.75E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.8E-5 1/K | ||
400.0 °C | 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | ||
Conductividad térmica | 20.0 °C | 15 W/(m·K) Show Material materials with Conductividad térmica of 15 W/(m·K) | |
Temperatura de fusión | 1425 - 1530 °C Show Material materials with Temperatura de fusión of 1425 - 1530 °C | Typical for Ferritic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.3E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.06 % Show Material materials with Carbono of 0.06 % |
Cromo | 18 - 20 % Show Material materials with Cromo of 18 - 20 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Nitrógeno | 0.12 - 0.22 % Show Material materials with Nitrógeno of 0.12 - 0.22 % |
Níquel | 8 - 11 % Show Material materials with Níquel of 8 - 11 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |