Mecánica
Property | Temperature | Value |
---|---|---|
Elongación A50 | 23.0 °C | 14 - 16 % Show Material materials with Elongación A50 of 14 - 16 % |
Estricción | 23.0 °C | 45 % Show Material materials with Estricción of 45 % |
Límite elástico | 23.0 °C | 620 - 690 MPa Show Material materials with Límite elástico of 620 - 690 MPa |
Resistencia a la tracción | 23.0 °C | 725 - 930 MPa Show Material materials with Resistencia a la tracción of 725 - 930 MPa |
Chemical properties
Property | Value |
---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Boro | 2.5E-3 % Show Material materials with Boro of 2.5E-3 % |
Carbono | 0.15 - 0.21 % Show Material materials with Carbono of 0.15 - 0.21 % |
Circonio | 0.05 - 0.15 % Show Material materials with Circonio of 0.05 - 0.15 % |
Cromo | 0.5 - 0.8 % Show Material materials with Cromo of 0.5 - 0.8 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.8 - 1.1 % Show Material materials with Manganeso of 0.8 - 1.1 % |
Molibdeno | 0.18 - 0.28 % Show Material materials with Molibdeno of 0.18 - 0.28 % |
Silicona | 0.4 - 0.8 % Show Material materials with Silicona of 0.4 - 0.8 % |