General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel |
Elongación A50 | 23.0 °C | 14 - 16 % Show Material materials with Elongación A50 of 14 - 16 % | |
Estricción | 23.0 °C | 45 % Show Material materials with Estricción of 45 % | |
Límite elástico | 23.0 °C | 620 - 690 MPa Show Material materials with Límite elástico of 620 - 690 MPa | |
Módulo elástico | 23.0 °C | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel |
Resistencia a la tracción | 23.0 °C | 725 - 930 MPa Show Material materials with Resistencia a la tracción of 725 - 930 MPa |
Chemical properties
Property | Value |
---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Boro | 1E-3 - 5E-3 % Show Material materials with Boro of 1E-3 - 5E-3 % |
Carbono | 0.12 - 0.21 % Show Material materials with Carbono of 0.12 - 0.21 % |
Cromo | 0.85 - 1.2 % Show Material materials with Cromo of 0.85 - 1.2 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.45 - 0.7 % Show Material materials with Manganeso of 0.45 - 0.7 % |
Molibdeno | 0.45 - 0.6 % Show Material materials with Molibdeno of 0.45 - 0.6 % |
Níquel | 1.2 - 1.5 % Show Material materials with Níquel of 1.2 - 1.5 % |
Silicona | 0.2 - 0.35 % Show Material materials with Silicona of 0.2 - 0.35 % |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % |