General
Property | Value | Comment |
---|---|---|
Densidad | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | |||
Dureza Brinell | 239 [-] Show Material materials with Dureza Brinell of 239 [-] | Predicted Value, Transverse | |||
Elongación | 17.9 % Show Material materials with Elongación of 17.9 % | Predicted Value, A80 | |||
18 % Show Material materials with Elongación of 18 % | Normalized | ASTM A537 | Plate | A200 | |
18.5 % Show Material materials with Elongación of 18.5 % | Predicted Value, Transverse | ||||
19.3 % Show Material materials with Elongación of 19.3 % | Predicted Value, A80 Transverse | ||||
22 % Show Material materials with Elongación of 22 % | Normalized | ASTM A537 | Plate | A50 | |
24.7 % Show Material materials with Elongación of 24.7 % | Predicted Value | ||||
Estricción | 40.6 % Show Material materials with Estricción of 40.6 % | Predicted Value | |||
43.9 % Show Material materials with Estricción of 43.9 % | Predicted Value, Transverse | ||||
Límite elástico | 264.2 MPa Show Material materials with Límite elástico of 264.2 MPa | Predicted Value, RP1 | |||
310 MPa Show Material materials with Límite elástico of 310 MPa | Normalized | ASTM A537 | Plate | ||
317.5 MPa Show Material materials with Límite elástico of 317.5 MPa | Predicted Value, RP1 Transverse | ||||
338.9 MPa Show Material materials with Límite elástico of 338.9 MPa | Predicted Value, RP05 | ||||
345 MPa Show Material materials with Límite elástico of 345 MPa | Normalized | ASTM A537 | Plate | ||
345.4 MPa Show Material materials with Límite elástico of 345.4 MPa | Predicted Value, Transverse | ||||
378 MPa Show Material materials with Límite elástico of 378 MPa | Predicted Value, RP02 | ||||
404.9 MPa Show Material materials with Límite elástico of 404.9 MPa | Predicted Value, RP002 | ||||
469.4 MPa Show Material materials with Límite elástico of 469.4 MPa | Predicted Value, RP02 Transverse | ||||
Módulo de cizallamiento | 79.6 GPa Show Material materials with Módulo de cizallamiento of 79.6 GPa | Predicted Value | |||
Módulo elástico | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel | |||
Resistencia a la tracción | 450 - 585 MPa Show Material materials with Resistencia a la tracción of 450 - 585 MPa | Normalized | ASTM A537 | Plate | |
485 - 620 MPa Show Material materials with Resistencia a la tracción of 485 - 620 MPa | Normalized | ASTM A537 | Plate | ||
Resistencia al cizallamiento | 534.1 MPa Show Material materials with Resistencia al cizallamiento of 534.1 MPa | Predicted Value |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 458 J/(kg·K) Show Material materials with Calor específico of 458 J/(kg·K) | Predicted Value |
Coeficiente de dilatación térmica | 11.94 1/K Show Material materials with Coeficiente de dilatación térmica of 11.94 1/K | Predicted Value |
Conductividad térmica | 32.64 W/(m·K) Show Material materials with Conductividad térmica of 32.64 W/(m·K) | Predicted Value |
Eléctrico
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % | Normalized | ASTM A537 | Plate |
Carbono | 0.24 % Show Material materials with Carbono of 0.24 % | Normalized | ASTM A537 | Plate |
Cobre | 0.35 % Show Material materials with Cobre of 0.35 % | Normalized | ASTM A537 | Plate |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | Normalized | ASTM A537 | Plate |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | Normalized | ASTM A537 | Plate |
Manganeso | 0.7 - 1.35 % Show Material materials with Manganeso of 0.7 - 1.35 % | Normalized | ASTM A537 | Plate |
Molibdeno | 0.08 % Show Material materials with Molibdeno of 0.08 % | Normalized | ASTM A537 | Plate |
Níquel | 0.25 % Show Material materials with Níquel of 0.25 % | Normalized | ASTM A537 | Plate |
Silicona | 0.15 - 0.5 % Show Material materials with Silicona of 0.15 - 0.5 % | Normalized | ASTM A537 | Plate |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |