General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.82 - 7.85 g/cm³ Show Material materials with Densidad of 7.82 - 7.85 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Medium Carbon Steel |
Dureza Rockwell C | 20.0 °C | 51 [-] Show Material materials with Dureza Rockwell C of 51 [-] | |
Dureza Vickers | 20.0 °C | 530 [-] Show Material materials with Dureza Vickers of 530 [-] | |
Módulo de cizallamiento | 20.0 °C | 81 GPa Show Material materials with Módulo de cizallamiento of 81 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 210 - 212 GPa Show Material materials with Módulo elástico of 210 - 212 GPa | ||
100.0 °C | 205 - 207 GPa Show Material materials with Módulo elástico of 205 - 207 GPa | ||
200.0 °C | 195 - 199 GPa Show Material materials with Módulo elástico of 195 - 199 GPa | ||
300.0 °C | 185 - 192 GPa Show Material materials with Módulo elástico of 185 - 192 GPa | ||
400.0 °C | 175 - 184 GPa Show Material materials with Módulo elástico of 175 - 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 - 480 J/(kg·K) Show Material materials with Calor específico of 461 - 480 J/(kg·K) | ||
100.0 °C | 479 - 500 J/(kg·K) Show Material materials with Calor específico of 479 - 500 J/(kg·K) | ||
200.0 °C | 499 - 550 J/(kg·K) Show Material materials with Calor específico of 499 - 550 J/(kg·K) | ||
300.0 °C | 517 - 590 J/(kg·K) Show Material materials with Calor específico of 517 - 590 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.11E-5 - 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.11E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.21E-5 - 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.29E-5 - 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.35E-5 - 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.35E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | ||
Conductividad térmica | 20.0 °C | 48 - 52 W/(m·K) Show Material materials with Conductividad térmica of 48 - 52 W/(m·K) | |
100.0 °C | 48.9 - 50.6 W/(m·K) Show Material materials with Conductividad térmica of 48.9 - 50.6 W/(m·K) | ||
200.0 °C | 47.5 - 48.1 W/(m·K) Show Material materials with Conductividad térmica of 47.5 - 48.1 W/(m·K) | ||
300.0 °C | 44.7 - 45.7 W/(m·K) Show Material materials with Conductividad térmica of 44.7 - 45.7 W/(m·K) | ||
400.0 °C | 41.6 W/(m·K) Show Material materials with Conductividad térmica of 41.6 W/(m·K) | ||
500.0 °C | 38.6 W/(m·K) Show Material materials with Conductividad térmica of 38.6 W/(m·K) | ||
600.0 °C | 35.5 W/(m·K) Show Material materials with Conductividad térmica of 35.5 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 13.3 mm²/s Show Material materials with Difusividad térmica of 13.3 mm²/s | |
100.0 °C | 12.6 mm²/s Show Material materials with Difusividad térmica of 12.6 mm²/s | ||
200.0 °C | 11.5 mm²/s Show Material materials with Difusividad térmica of 11.5 mm²/s | ||
300.0 °C | 10.2 mm²/s Show Material materials with Difusividad térmica of 10.2 mm²/s | ||
400.0 °C | 8.9 mm²/s Show Material materials with Difusividad térmica of 8.9 mm²/s | ||
500.0 °C | 7.5 mm²/s Show Material materials with Difusividad térmica of 7.5 mm²/s | ||
600.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
Temperatura de fusión | 1380 - 1514 °C Show Material materials with Temperatura de fusión of 1380 - 1514 °C | Typical for Medium Carbon Steel | |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.2E-7 - 2.17E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.2E-7 - 2.17E-7 Ω·m |
100.0 °C | 2.62E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.62E-7 Ω·m | |
200.0 °C | 3.32E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.32E-7 Ω·m | |
300.0 °C | 4.2E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.2E-7 Ω·m | |
400.0 °C | 5.23E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.23E-7 Ω·m | |
500.0 °C | 6.41E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.41E-7 Ω·m | |
600.0 °C | 7.8E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.8E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % |
Carbono | 0.37 - 0.44 % Show Material materials with Carbono of 0.37 - 0.44 % |
Cromo | 0.4 % Show Material materials with Cromo of 0.4 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.5 - 0.8 % Show Material materials with Manganeso of 0.5 - 0.8 % |
Molibdeno | 0.1 % Show Material materials with Molibdeno of 0.1 % |
Níquel | 0.4 % Show Material materials with Níquel of 0.4 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |