Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) |
0.0 °C | 456 J/(kg·K) Show Material materials with Calor específico of 456 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | |
Coeficiente de dilatación térmica | -100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K |
0.0 °C | 1.14E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.14E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | |
100.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | |
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | |
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | |
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | |
500.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | |
600.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | |
Conductividad térmica | -100.0 °C | 31.9 W/(m·K) Show Material materials with Conductividad térmica of 31.9 W/(m·K) |
0.0 °C | 36.9 W/(m·K) Show Material materials with Conductividad térmica of 36.9 W/(m·K) | |
20.0 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | |
100.0 °C | 39.3 W/(m·K) Show Material materials with Conductividad térmica of 39.3 W/(m·K) | |
200.0 °C | 40.1 W/(m·K) Show Material materials with Conductividad térmica of 40.1 W/(m·K) | |
300.0 °C | 39.6 W/(m·K) Show Material materials with Conductividad térmica of 39.6 W/(m·K) | |
400.0 °C | 38.4 W/(m·K) Show Material materials with Conductividad térmica of 38.4 W/(m·K) | |
500.0 °C | 36.7 W/(m·K) Show Material materials with Conductividad térmica of 36.7 W/(m·K) | |
600.0 °C | 34.8 W/(m·K) Show Material materials with Conductividad térmica of 34.8 W/(m·K) | |
Difusividad térmica | -100.0 °C | 10900 mm²/s Show Material materials with Difusividad térmica of 10900 mm²/s |
0.0 °C | 10400 mm²/s Show Material materials with Difusividad térmica of 10400 mm²/s | |
20.0 °C | 10400 mm²/s Show Material materials with Difusividad térmica of 10400 mm²/s | |
100.0 °C | 10100 mm²/s Show Material materials with Difusividad térmica of 10100 mm²/s | |
200.0 °C | 9700 mm²/s Show Material materials with Difusividad térmica of 9700 mm²/s | |
300.0 °C | 9000 mm²/s Show Material materials with Difusividad térmica of 9000 mm²/s | |
400.0 °C | 8100 mm²/s Show Material materials with Difusividad térmica of 8100 mm²/s | |
500.0 °C | 7100 mm²/s Show Material materials with Difusividad térmica of 7100 mm²/s | |
600.0 °C | 5900 mm²/s Show Material materials with Difusividad térmica of 5900 mm²/s | |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | -100.0 °C | 2.14E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.14E-7 Ω·m |
0.0 °C | 2.66E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.66E-7 Ω·m | |
20.0 °C | 2.77E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.77E-7 Ω·m | |
100.0 °C | 3.26E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.26E-7 Ω·m | |
200.0 °C | 3.94E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.94E-7 Ω·m | |
300.0 °C | 4.74E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.74E-7 Ω·m | |
400.0 °C | 5.66E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.66E-7 Ω·m | |
500.0 °C | 6.73E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.73E-7 Ω·m | |
600.0 °C | 7.96E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.96E-7 Ω·m | |
General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.84 - 7.85 g/cm³ Show Material materials with Densidad of 7.84 - 7.85 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 229 [-] Show Material materials with Dureza Brinell of 229 [-] |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa |
0.0 °C | 213 GPa Show Material materials with Módulo elástico of 213 GPa | |
20.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | |
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | |
200.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | |
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | |
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | |
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % |
Carbono | 0.15 - 0.2 % Show Material materials with Carbono of 0.15 - 0.2 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 1.5 - 1.8 % Show Material materials with Cromo of 1.5 - 1.8 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.4 - 0.6 % Show Material materials with Manganeso of 0.4 - 0.6 % |
Molibdeno | 0.25 - 0.35 % Show Material materials with Molibdeno of 0.25 - 0.35 % |
Níquel | 1.4 - 1.7 % Show Material materials with Níquel of 1.4 - 1.7 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |