General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel |
Elongación A50 | 23.0 °C | 16 - 18 % Show Material materials with Elongación A50 of 16 - 18 % | |
Límite elástico Rp 0,2 | 23.0 °C | 620 - 690 MPa Show Material materials with Límite elástico Rp 0,2 of 620 - 690 MPa | |
Módulo elástico | 23.0 °C | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel |
Resistencia a la tracción | 23.0 °C | 690 - 895 MPa Show Material materials with Resistencia a la tracción of 690 - 895 MPa |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.02 - 0.05 % Show Material materials with Aluminio of 0.02 - 0.05 % |
Azufre | 6E-3 % Show Material materials with Azufre of 6E-3 % |
Carbono | 0.08 % Show Material materials with Carbono of 0.08 % |
Cobre | 0.9 - 1.2 % Show Material materials with Cobre of 0.9 - 1.2 % |
Cromo | 0.4 - 0.65 % Show Material materials with Cromo of 0.4 - 0.65 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Manganeso | 0.95 - 1.5 % Show Material materials with Manganeso of 0.95 - 1.5 % |
Molibdeno | 0.4 - 0.65 % Show Material materials with Molibdeno of 0.4 - 0.65 % |
Niobio | 0.01 - 0.03 % Show Material materials with Niobio of 0.01 - 0.03 % |
Nitrógeno | 0.02 % Show Material materials with Nitrógeno of 0.02 % |
Níquel | 0.65 - 0.9 % Show Material materials with Níquel of 0.65 - 0.9 % |
Silicona | 0.15 - 0.35 % Show Material materials with Silicona of 0.15 - 0.35 % |
Vanadio | 0.04 - 0.08 % Show Material materials with Vanadio of 0.04 - 0.08 % |