General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel |
Elongación A50 | 23.0 °C | 25 % Show Material materials with Elongación A50 of 25 % | |
Estricción | 23.0 °C | 45 % Show Material materials with Estricción of 45 % | |
Límite elástico Rp 0,2 | 23.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | |
Módulo elástico | 23.0 °C | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel |
Resistencia a la tracción | 23.0 °C | 750 - 895 MPa Show Material materials with Resistencia a la tracción of 750 - 895 MPa |
Chemical properties
Property | Value |
---|---|
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cromo | 24 - 26 % Show Material materials with Cromo of 24 - 26 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Molibdeno | 2.5 - 3.5 % Show Material materials with Molibdeno of 2.5 - 3.5 % |
Níquel | 6 - 8 % Show Material materials with Níquel of 6 - 8 % |
Silicona | 0.8 % Show Material materials with Silicona of 0.8 % |