General
Property | Value | Comment |
---|---|---|
Densidad | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
Dureza Brinell | 249 [-] Show Material materials with Dureza Brinell of 249 [-] | Predicted Value, Transverse | ||||
Elongación | 18.4 % Show Material materials with Elongación of 18.4 % | Predicted Value, A200 | ||||
21.4 % Show Material materials with Elongación of 21.4 % | Predicted Value, A5 | |||||
26.6 % Show Material materials with Elongación of 26.6 % | Predicted Value, A50 | |||||
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 23 % Show Material materials with Elongación of 23 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 24 % Show Material materials with Elongación of 24 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 24 % Show Material materials with Elongación of 24 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 26 % Show Material materials with Elongación of 26 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Estricción | 44.1 % Show Material materials with Estricción of 44.1 % | Predicted Value, Transverse | ||||
50.8 % Show Material materials with Estricción of 50.8 % | Predicted Value | |||||
Límite elástico | 263.7 MPa Show Material materials with Límite elástico of 263.7 MPa | Predicted Value, RP1 | ||||
269.2 MPa Show Material materials with Límite elástico of 269.2 MPa | Predicted Value, RP05 | |||||
278.1 MPa Show Material materials with Límite elástico of 278.1 MPa | Predicted Value, Transverse | |||||
320.4 MPa Show Material materials with Límite elástico of 320.4 MPa | Predicted Value, RP1 Transverse | |||||
349.1 MPa Show Material materials with Límite elástico of 349.1 MPa | Predicted Value, RP02 | |||||
445.3 MPa Show Material materials with Límite elástico of 445.3 MPa | Predicted Value, RP02 Transverse | |||||
468.1 MPa Show Material materials with Límite elástico of 468.1 MPa | Predicted Value, RP002 | |||||
20 °C | 165 MPa Show Material materials with Límite elástico of 165 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 175 MPa Show Material materials with Límite elástico of 175 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 185 MPa Show Material materials with Límite elástico of 185 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 195 MPa Show Material materials with Límite elástico of 195 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 159 - 187 MPa Show Material materials with Límite elástico of 159 - 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 159 - 180 MPa Show Material materials with Límite elástico of 159 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 159 - 173 MPa Show Material materials with Límite elástico of 159 - 173 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 159 MPa Show Material materials with Límite elástico of 159 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 173 - 187 MPa Show Material materials with Límite elástico of 173 - 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 173 - 180 MPa Show Material materials with Límite elástico of 173 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 173 MPa Show Material materials with Límite elástico of 173 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 - 187 MPa Show Material materials with Límite elástico of 180 - 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 MPa Show Material materials with Límite elástico of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 187 MPa Show Material materials with Límite elástico of 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 - 161 MPa Show Material materials with Límite elástico of 137 - 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 - 155 MPa Show Material materials with Límite elástico of 137 - 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 - 149 MPa Show Material materials with Límite elástico of 137 - 149 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 MPa Show Material materials with Límite elástico of 137 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 149 - 161 MPa Show Material materials with Límite elástico of 149 - 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 149 - 155 MPa Show Material materials with Límite elástico of 149 - 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 149 MPa Show Material materials with Límite elástico of 149 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 161 MPa Show Material materials with Límite elástico of 155 - 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 MPa Show Material materials with Límite elástico of 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 161 MPa Show Material materials with Límite elástico of 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 - 143 MPa Show Material materials with Límite elástico of 115 - 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 - 136 MPa Show Material materials with Límite elástico of 115 - 136 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 - 129 MPa Show Material materials with Límite elástico of 115 - 129 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 MPa Show Material materials with Límite elástico of 115 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 129 - 143 MPa Show Material materials with Límite elástico of 129 - 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 129 - 136 MPa Show Material materials with Límite elástico of 129 - 136 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 129 MPa Show Material materials with Límite elástico of 129 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 136 - 143 MPa Show Material materials with Límite elástico of 136 - 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 136 MPa Show Material materials with Límite elástico of 136 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 143 MPa Show Material materials with Límite elástico of 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 - 122 MPa Show Material materials with Límite elástico of 102 - 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 - 117 MPa Show Material materials with Límite elástico of 102 - 117 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 - 112 MPa Show Material materials with Límite elástico of 102 - 112 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 MPa Show Material materials with Límite elástico of 102 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 112 - 122 MPa Show Material materials with Límite elástico of 112 - 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 112 - 117 MPa Show Material materials with Límite elástico of 112 - 117 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 112 MPa Show Material materials with Límite elástico of 112 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 117 - 122 MPa Show Material materials with Límite elástico of 117 - 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 117 MPa Show Material materials with Límite elástico of 117 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 122 MPa Show Material materials with Límite elástico of 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | 200 - 215 GPa Show Material materials with Módulo elástico of 200 - 215 GPa | Typical for Low Carbon Steel | ||||
Resistencia a la tracción | 20 °C | 330 - 510 MPa Show Material materials with Resistencia a la tracción of 330 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 330 - 500 MPa Show Material materials with Resistencia a la tracción of 330 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 330 - 490 MPa Show Material materials with Resistencia a la tracción of 330 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 330 - 480 MPa Show Material materials with Resistencia a la tracción of 330 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 510 MPa Show Material materials with Resistencia a la tracción of 340 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 500 MPa Show Material materials with Resistencia a la tracción of 340 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 490 MPa Show Material materials with Resistencia a la tracción of 340 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 480 MPa Show Material materials with Resistencia a la tracción of 340 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 510 MPa Show Material materials with Resistencia a la tracción of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 500 MPa Show Material materials with Resistencia a la tracción of 350 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 490 MPa Show Material materials with Resistencia a la tracción of 350 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 480 MPa Show Material materials with Resistencia a la tracción of 350 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 510 MPa Show Material materials with Resistencia a la tracción of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 500 MPa Show Material materials with Resistencia a la tracción of 360 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 490 MPa Show Material materials with Resistencia a la tracción of 360 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 480 MPa Show Material materials with Resistencia a la tracción of 360 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia al cizallamiento | 511.9 MPa Show Material materials with Resistencia al cizallamiento of 511.9 MPa | Predicted Value |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 465 J/(kg·K) Show Material materials with Calor específico of 465 J/(kg·K) | Typical for Low Carbon Steel |
Coeficiente de dilatación térmica | 1.32e-05 - 1.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 - 1.38e-05 1/K | Typical for Low Carbon Steel |
Conductividad térmica | 25 - 93 W/(m·K) Show Material materials with Conductividad térmica of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel |
Temperatura máx. de funcionamiento | 294.5 °C Show Material materials with Temperatura máx. de funcionamiento of 294.5 °C | Predicted Value, Long |
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 7 S/m Show Material materials with Conductividad eléctrica of 7 S/m | Predicted Value |
Resistividad eléctrica | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Carbono | 0.17 % Show Material materials with Carbono of 0.17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Cobre | 0.55 % Show Material materials with Cobre of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Manganeso | 1.4 % Show Material materials with Manganeso of 1.4 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |