General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 244 [-] Show Material materials with Dureza Brinell of 244 [-] | Predicted Value, Transverse | ||||
Elongación | 17.6 % Show Material materials with Elongación of 17.6 % | Predicted Value, A200 | ||||
19.6 % Show Material materials with Elongación of 19.6 % | Predicted Value, A50 | |||||
22.4 % Show Material materials with Elongación of 22.4 % | Predicted Value, A5 | |||||
20 °C | 12 % Show Material materials with Elongación of 12 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 13 % Show Material materials with Elongación of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Estricción | 44.3 % Show Material materials with Estricción of 44.3 % | Predicted Value, Transverse | ||||
51.9 % Show Material materials with Estricción of 51.9 % | Predicted Value | |||||
Límite elástico | 243.8 MPa Show Material materials with Límite elástico of 243.8 MPa | Predicted Value, RP1 | ||||
309.1 MPa Show Material materials with Límite elástico of 309.1 MPa | Predicted Value, RP1 Transverse | |||||
368.5 MPa Show Material materials with Límite elástico of 368.5 MPa | Predicted Value, Transverse | |||||
383.4 MPa Show Material materials with Límite elástico of 383.4 MPa | Predicted Value, RP05 | |||||
400.2 MPa Show Material materials with Límite elástico of 400.2 MPa | Predicted Value, RP02 | |||||
475.2 MPa Show Material materials with Límite elástico of 475.2 MPa | Predicted Value, RP02 Transverse | |||||
480.2 MPa Show Material materials with Límite elástico of 480.2 MPa | Predicted Value, RP002 | |||||
20 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 325 MPa Show Material materials with Límite elástico of 325 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia a la tracción | 20 °C | 450 - 680 MPa Show Material materials with Resistencia a la tracción of 450 - 680 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 450 - 630 MPa Show Material materials with Resistencia a la tracción of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 450 - 600 MPa Show Material materials with Resistencia a la tracción of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 680 MPa Show Material materials with Resistencia a la tracción of 470 - 680 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 600 MPa Show Material materials with Resistencia a la tracción of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 680 MPa Show Material materials with Resistencia a la tracción of 510 - 680 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 630 MPa Show Material materials with Resistencia a la tracción of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 600 MPa Show Material materials with Resistencia a la tracción of 510 - 600 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia al cizallamiento | 508.4 MPa Show Material materials with Resistencia al cizallamiento of 508.4 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Conductividad térmica | 20 °C | 46.5 W/(m·K) Show Material materials with Conductividad térmica of 46.5 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 47.2 W/(m·K) Show Material materials with Conductividad térmica of 47.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 45.9 W/(m·K) Show Material materials with Conductividad térmica of 45.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 43.5 W/(m·K) Show Material materials with Conductividad térmica of 43.5 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 40.9 W/(m·K) Show Material materials with Conductividad térmica of 40.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 38.1 W/(m·K) Show Material materials with Conductividad térmica of 38.1 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 35.3 W/(m·K) Show Material materials with Conductividad térmica of 35.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Difusividad térmica | 20 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 12.2 mm²/s Show Material materials with Difusividad térmica of 12.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 11.1 mm²/s Show Material materials with Difusividad térmica of 11.1 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 9.9 mm²/s Show Material materials with Difusividad térmica of 9.9 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 8.7 mm²/s Show Material materials with Difusividad térmica of 8.7 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 368.8 °C Show Material materials with Temperatura máx. de funcionamiento of 368.8 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 7 S/m Show Material materials with Conductividad eléctrica of 7 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 2.24e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.24e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 2.71e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.71e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 3.44e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.44e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 4.31e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.31e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 5.32e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.32e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 6.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 7.86e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.86e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Cobre | 0.55 % Show Material materials with Cobre of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Manganeso | 1.6 % Show Material materials with Manganeso of 1.6 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Silicona | 0.55 % Show Material materials with Silicona of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |