General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 243 [-] Show Material materials with Dureza Brinell of 243 [-] | Predicted Value, Transverse | ||||
Elongación | 17.7 % Show Material materials with Elongación of 17.7 % | Predicted Value, A200 | ||||
19.6 % Show Material materials with Elongación of 19.6 % | Predicted Value, A50 | |||||
22.3 % Show Material materials with Elongación of 22.3 % | Predicted Value, A5 | |||||
20 °C | 12 % Show Material materials with Elongación of 12 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 13 % Show Material materials with Elongación of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Estricción | 44.0 % Show Material materials with Estricción of 44.0 % | Predicted Value, Transverse | ||||
52.7 % Show Material materials with Estricción of 52.7 % | Predicted Value | |||||
Límite elástico | 243.9 MPa Show Material materials with Límite elástico of 243.9 MPa | Predicted Value, RP1 | ||||
308.5 MPa Show Material materials with Límite elástico of 308.5 MPa | Predicted Value, RP1 Transverse | |||||
367.7 MPa Show Material materials with Límite elástico of 367.7 MPa | Predicted Value, Transverse | |||||
379.8 MPa Show Material materials with Límite elástico of 379.8 MPa | Predicted Value, RP05 | |||||
420.8 MPa Show Material materials with Límite elástico of 420.8 MPa | Predicted Value, RP02 | |||||
477.7 MPa Show Material materials with Límite elástico of 477.7 MPa | Predicted Value, RP02 Transverse | |||||
480.2 MPa Show Material materials with Límite elástico of 480.2 MPa | Predicted Value, RP002 | |||||
20 °C | 265 MPa Show Material materials with Límite elástico of 265 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 285 MPa Show Material materials with Límite elástico of 285 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 315 MPa Show Material materials with Límite elástico of 315 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 325 MPa Show Material materials with Límite elástico of 325 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 335 MPa Show Material materials with Límite elástico of 335 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 355 MPa Show Material materials with Límite elástico of 355 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 194 - 254 MPa Show Material materials with Límite elástico of 194 - 254 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 194 - 249 MPa Show Material materials with Límite elástico of 194 - 249 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 194 - 234 MPa Show Material materials with Límite elástico of 194 - 234 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 194 - 224 MPa Show Material materials with Límite elástico of 194 - 224 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 194 - 214 MPa Show Material materials with Límite elástico of 194 - 214 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 194 MPa Show Material materials with Límite elástico of 194 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 214 - 254 MPa Show Material materials with Límite elástico of 214 - 254 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 214 - 249 MPa Show Material materials with Límite elástico of 214 - 249 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 214 - 234 MPa Show Material materials with Límite elástico of 214 - 234 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 214 - 224 MPa Show Material materials with Límite elástico of 214 - 224 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 214 MPa Show Material materials with Límite elástico of 214 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 224 - 254 MPa Show Material materials with Límite elástico of 224 - 254 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 224 - 249 MPa Show Material materials with Límite elástico of 224 - 249 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 224 - 234 MPa Show Material materials with Límite elástico of 224 - 234 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 224 MPa Show Material materials with Límite elástico of 224 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 234 - 254 MPa Show Material materials with Límite elástico of 234 - 254 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 234 - 249 MPa Show Material materials with Límite elástico of 234 - 249 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 234 MPa Show Material materials with Límite elástico of 234 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 249 - 254 MPa Show Material materials with Límite elástico of 249 - 254 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 249 MPa Show Material materials with Límite elástico of 249 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 254 MPa Show Material materials with Límite elástico of 254 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 166 - 226 MPa Show Material materials with Límite elástico of 166 - 226 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 166 - 221 MPa Show Material materials with Límite elástico of 166 - 221 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 166 - 206 MPa Show Material materials with Límite elástico of 166 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 166 - 196 MPa Show Material materials with Límite elástico of 166 - 196 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 166 - 186 MPa Show Material materials with Límite elástico of 166 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 166 MPa Show Material materials with Límite elástico of 166 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 186 - 226 MPa Show Material materials with Límite elástico of 186 - 226 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 186 - 221 MPa Show Material materials with Límite elástico of 186 - 221 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 186 - 206 MPa Show Material materials with Límite elástico of 186 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 186 - 196 MPa Show Material materials with Límite elástico of 186 - 196 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 186 MPa Show Material materials with Límite elástico of 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 196 - 226 MPa Show Material materials with Límite elástico of 196 - 226 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 196 - 221 MPa Show Material materials with Límite elástico of 196 - 221 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 196 - 206 MPa Show Material materials with Límite elástico of 196 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 196 MPa Show Material materials with Límite elástico of 196 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 206 - 226 MPa Show Material materials with Límite elástico of 206 - 226 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 206 - 221 MPa Show Material materials with Límite elástico of 206 - 221 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 206 MPa Show Material materials with Límite elástico of 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 221 - 226 MPa Show Material materials with Límite elástico of 221 - 226 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 221 MPa Show Material materials with Límite elástico of 221 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 226 MPa Show Material materials with Límite elástico of 226 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 146 - 206 MPa Show Material materials with Límite elástico of 146 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 146 - 202 MPa Show Material materials with Límite elástico of 146 - 202 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 146 - 186 MPa Show Material materials with Límite elástico of 146 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 146 - 176 MPa Show Material materials with Límite elástico of 146 - 176 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 146 - 166 MPa Show Material materials with Límite elástico of 146 - 166 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 146 MPa Show Material materials with Límite elástico of 146 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 166 - 206 MPa Show Material materials with Límite elástico of 166 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 166 - 186 MPa Show Material materials with Límite elástico of 166 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 166 MPa Show Material materials with Límite elástico of 166 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 166 - 202 MPa Show Material materials with Límite elástico of 166 - 202 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 166 - 176 MPa Show Material materials with Límite elástico of 166 - 176 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 176 - 206 MPa Show Material materials with Límite elástico of 176 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 176 - 202 MPa Show Material materials with Límite elástico of 176 - 202 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 176 - 186 MPa Show Material materials with Límite elástico of 176 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 176 MPa Show Material materials with Límite elástico of 176 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 186 - 206 MPa Show Material materials with Límite elástico of 186 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 186 MPa Show Material materials with Límite elástico of 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 186 - 202 MPa Show Material materials with Límite elástico of 186 - 202 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 202 - 206 MPa Show Material materials with Límite elástico of 202 - 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 202 MPa Show Material materials with Límite elástico of 202 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 206 MPa Show Material materials with Límite elástico of 206 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 126 - 186 MPa Show Material materials with Límite elástico of 126 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 126 - 181 MPa Show Material materials with Límite elástico of 126 - 181 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 126 - 166 MPa Show Material materials with Límite elástico of 126 - 166 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 126 - 156 MPa Show Material materials with Límite elástico of 126 - 156 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 126 - 146 MPa Show Material materials with Límite elástico of 126 - 146 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 126 MPa Show Material materials with Límite elástico of 126 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 146 - 186 MPa Show Material materials with Límite elástico of 146 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 146 - 166 MPa Show Material materials with Límite elástico of 146 - 166 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 146 MPa Show Material materials with Límite elástico of 146 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 146 - 181 MPa Show Material materials with Límite elástico of 146 - 181 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 146 - 156 MPa Show Material materials with Límite elástico of 146 - 156 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 156 - 186 MPa Show Material materials with Límite elástico of 156 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 156 - 181 MPa Show Material materials with Límite elástico of 156 - 181 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 156 - 166 MPa Show Material materials with Límite elástico of 156 - 166 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 156 MPa Show Material materials with Límite elástico of 156 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 166 - 186 MPa Show Material materials with Límite elástico of 166 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 166 MPa Show Material materials with Límite elástico of 166 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 166 - 181 MPa Show Material materials with Límite elástico of 166 - 181 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 181 - 186 MPa Show Material materials with Límite elástico of 181 - 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 181 MPa Show Material materials with Límite elástico of 181 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 186 MPa Show Material materials with Límite elástico of 186 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia a la tracción | 20 °C | 450 - 680 MPa Show Material materials with Resistencia a la tracción of 450 - 680 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 450 - 630 MPa Show Material materials with Resistencia a la tracción of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 450 - 600 MPa Show Material materials with Resistencia a la tracción of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 680 MPa Show Material materials with Resistencia a la tracción of 470 - 680 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 630 MPa Show Material materials with Resistencia a la tracción of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 470 - 600 MPa Show Material materials with Resistencia a la tracción of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 680 MPa Show Material materials with Resistencia a la tracción of 510 - 680 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 630 MPa Show Material materials with Resistencia a la tracción of 510 - 630 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 600 MPa Show Material materials with Resistencia a la tracción of 510 - 600 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia al cizallamiento | 513.8 MPa Show Material materials with Resistencia al cizallamiento of 513.8 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Conductividad térmica | -100 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 42.2 W/(m·K) Show Material materials with Conductividad térmica of 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 43.2 W/(m·K) Show Material materials with Conductividad térmica of 43.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 42.9 W/(m·K) Show Material materials with Conductividad térmica of 42.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 41.2 W/(m·K) Show Material materials with Conductividad térmica of 41.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 39.1 W/(m·K) Show Material materials with Conductividad térmica of 39.1 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 36.6 W/(m·K) Show Material materials with Conductividad térmica of 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 34.1 W/(m·K) Show Material materials with Conductividad térmica of 34.1 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Difusividad térmica | -100 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 11.7 mm²/s Show Material materials with Difusividad térmica of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 9.4 mm²/s Show Material materials with Difusividad térmica of 9.4 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 305.4 °C Show Material materials with Temperatura máx. de funcionamiento of 305.4 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 7 S/m Show Material materials with Conductividad eléctrica of 7 S/m | Predicted Value | ||||
Resistividad eléctrica | -100 °C | 1.82e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.82e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 2.47e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.47e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 2.96e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.96e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 3.68e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 4.55e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 5.56e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 6.75e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.75e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 8.13e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Cobre | 0.55 % Show Material materials with Cobre of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Manganeso | 1.6 % Show Material materials with Manganeso of 1.6 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Silicona | 0.55 % Show Material materials with Silicona of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Technological properties
Property | ||
---|---|---|