General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.89 - 8.9 g/cm³ Show Material materials with Densidad of 8.89 - 8.9 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] |
Dureza Vickers | 20.0 °C | 140 - 170 [-] Show Material materials with Dureza Vickers of 140 - 170 [-] |
Módulo elástico | 20.0 °C | 140 GPa Show Material materials with Módulo elástico of 140 GPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 370 J/(kg·K) Show Material materials with Calor específico of 370 J/(kg·K) | |
100.0 °C | 390 J/(kg·K) Show Material materials with Calor específico of 390 J/(kg·K) | ||
200.0 °C | 410 J/(kg·K) Show Material materials with Calor específico of 410 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100.0 °C | 1.55E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.55E-5 1/K | |
200.0 °C | 1.59E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.59E-5 1/K | ||
300.0 °C | 1.66E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.66E-5 1/K | ||
Conductividad térmica | 20.0 °C | 48 W/(m·K) Show Material materials with Conductividad térmica of 48 W/(m·K) | |
100.0 °C | 56 W/(m·K) Show Material materials with Conductividad térmica of 56 W/(m·K) | ||
200.0 °C | 65 W/(m·K) Show Material materials with Conductividad térmica of 65 W/(m·K) | ||
Temperatura de fusión | 915 - 1240 °C Show Material materials with Temperatura de fusión of 915 - 1240 °C | Typical for Wrought Copper Nickel Grade |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 20.0 °C | 6.00E+6 - 6.40E+6 S/m Show Material materials with Conductividad eléctrica of 6.00E+6 - 6.40E+6 S/m |
Specific Electrical conductivity | 10 - 11 % IACS Show Material materials with Specific Electrical conductivity of 10 - 11 % IACS |
Chemical properties
Property | Value |
---|---|
Estaño | 1.8 - 2.8 % Show Material materials with Estaño of 1.8 - 2.8 % |
Hierro | 0.3 % Show Material materials with Hierro of 0.3 % |
Manganeso | 0.3 % Show Material materials with Manganeso of 0.3 % |
Níquel | 8.5 - 10.5 % Show Material materials with Níquel of 8.5 - 10.5 % |
Plomo | 0.03 % Show Material materials with Plomo of 0.03 % |
Zinc | 0.05 - 0.1 % Show Material materials with Zinc of 0.05 - 0.1 % |