General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.33 - 8.4 g/cm³ Show Material materials with Densidad of 8.33 - 8.4 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Vickers | 20.0 °C | 110 [-] Show Material materials with Dureza Vickers of 110 [-] |
Elongación | 20.0 °C | 25 - 45 % Show Material materials with Elongación of 25 - 45 % |
Elongación transversal | 20.0 °C | 35 % Show Material materials with Elongación transversal of 35 % |
Límite elástico Rp 0,2 | 10.0 °C | 230 MPa Show Material materials with Límite elástico Rp 0,2 of 230 MPa |
20.0 °C | 150 - 240 MPa Show Material materials with Límite elástico Rp 0,2 of 150 - 240 MPa | |
50.0 °C | 240 MPa Show Material materials with Límite elástico Rp 0,2 of 240 MPa | |
100.0 °C | 230 MPa Show Material materials with Límite elástico Rp 0,2 of 230 MPa | |
150.0 °C | 225 MPa Show Material materials with Límite elástico Rp 0,2 of 225 MPa | |
Límite elástico Rp 1,0 | 20.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa |
50.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa | |
100.0 °C | 148 MPa Show Material materials with Límite elástico Rp 1,0 of 148 MPa | |
150.0 °C | 143 MPa Show Material materials with Límite elástico Rp 1,0 of 143 MPa | |
200.0 °C | 138 MPa Show Material materials with Límite elástico Rp 1,0 of 138 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 240 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 240 MPa |
50.0 °C | 240 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 240 MPa | |
100.0 °C | 230 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 230 MPa | |
150.0 °C | 225 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 225 MPa | |
Módulo de cizallamiento | 20.0 °C | 42 GPa Show Material materials with Módulo de cizallamiento of 42 GPa |
Módulo elástico | 20.0 °C | 110 - 112 GPa Show Material materials with Módulo elástico of 110 - 112 GPa |
50.0 °C | 110 - 130 GPa Show Material materials with Módulo elástico of 110 - 130 GPa | |
100.0 °C | 108 - 128 GPa Show Material materials with Módulo elástico of 108 - 128 GPa | |
150.0 °C | 107 - 126 GPa Show Material materials with Módulo elástico of 107 - 126 GPa | |
200.0 °C | 106 - 123 GPa Show Material materials with Módulo elástico of 106 - 123 GPa | |
250.0 °C | 105 - 120 GPa Show Material materials with Módulo elástico of 105 - 120 GPa | |
300.0 °C | 118 GPa Show Material materials with Módulo elástico of 118 GPa | |
350.0 °C | 115 GPa Show Material materials with Módulo elástico of 115 GPa | |
400.0 °C | 112 GPa Show Material materials with Módulo elástico of 112 GPa | |
450.0 °C | 109 GPa Show Material materials with Módulo elástico of 109 GPa | |
500.0 °C | 105 GPa Show Material materials with Módulo elástico of 105 GPa | |
Resistencia a la tracción | 20.0 °C | 390 MPa Show Material materials with Resistencia a la tracción of 390 MPa |
Resistencia a la tracción transversal | 20.0 °C | 390 MPa Show Material materials with Resistencia a la tracción transversal of 390 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 377 J/(kg·K) Show Material materials with Calor específico of 377 J/(kg·K) | |
Coeficiente de dilatación térmica | 200.0 °C | 1.85E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.85E-5 1/K | |
Conductividad térmica | 20.0 °C | 100 W/(m·K) Show Material materials with Conductividad térmica of 100 W/(m·K) | |
Temperatura de fusión | 875 - 1075 °C Show Material materials with Temperatura de fusión of 875 - 1075 °C | Typical for Wrought Copper Brass |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 20.0 °C | 1.34E+7 S/m Show Material materials with Conductividad eléctrica of 1.34E+7 S/m |
Resistividad eléctrica | 20.0 °C | 7.5E-8 Ω·m Show Material materials with Resistividad eléctrica of 7.5E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminio | 1.8 - 2.3 % Show Material materials with Aluminio of 1.8 - 2.3 % |
Arsénico | 0.02 - 0.06 % Show Material materials with Arsénico of 0.02 - 0.06 % |
Cobre | 76 - 79 % Show Material materials with Cobre of 76 - 79 % |
Fósforo | 0.01 % Show Material materials with Fósforo of 0.01 % |
Hierro | 0.07 % Show Material materials with Hierro of 0.07 % |
Magnesio | 5E-3 % Show Material materials with Magnesio of 5E-3 % |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % |
Níquel | 0.1 % Show Material materials with Níquel of 0.1 % |
Plomo | 0.05 - 0.07 % Show Material materials with Plomo of 0.05 - 0.07 % |