General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.4 g/cm³ Show Material materials with Densidad of 7.4 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Leaded Phosphor Bronze |
Dureza Vickers | 20.0 °C | 125 [-] Show Material materials with Dureza Vickers of 125 [-] | |
Elongación | 20.0 °C | 20 % Show Material materials with Elongación of 20 % | |
Límite elástico Rp 0,2 | 20.0 °C | 180 MPa Show Material materials with Límite elástico Rp 0,2 of 180 MPa | |
Módulo elástico | 23.0 °C | 110 - 130 GPa Show Material materials with Módulo elástico of 110 - 130 GPa | Typical for Leaded Phosphor Bronze |
Resistencia a la tracción | 20.0 °C | 490 MPa Show Material materials with Resistencia a la tracción of 490 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 380 J/(kg·K) Show Material materials with Calor específico of 380 J/(kg·K) | Typical for Leaded Phosphor Bronze |
Coeficiente de dilatación térmica | 23.0 °C | 1.5E-5 - 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.5E-5 - 1.9E-5 1/K | Typical for Leaded Phosphor Bronze |
Chemical properties
Property | Value |
---|---|
Aluminio | 8 - 9.5 % Show Material materials with Aluminio of 8 - 9.5 % |
Estaño | 0.1 % Show Material materials with Estaño of 0.1 % |
Hierro | 1 - 3 % Show Material materials with Hierro of 1 - 3 % |
Manganeso | 2.5 % Show Material materials with Manganeso of 2.5 % |
Níquel | 2 - 4 % Show Material materials with Níquel of 2 - 4 % |
Plomo | 0.05 % Show Material materials with Plomo of 0.05 % |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % |