General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.79 - 8.8 g/cm³ Show Material materials with Densidad of 8.79 - 8.8 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] |
Elongación | 20.0 °C | 28 - 45 % Show Material materials with Elongación of 28 - 45 % |
Elongation A10 | 20.0 °C | 25 % Show Material materials with Elongation A10 of 25 % |
Elongation A100 | 20.0 °C | 20 % Show Material materials with Elongation A100 of 20 % |
Elongation A11.3 | 20.0 °C | 40 % Show Material materials with Elongation A11.3 of 40 % |
Límite elástico Rp 0,2 | 20.0 °C | 80 - 150 MPa Show Material materials with Límite elástico Rp 0,2 of 80 - 150 MPa |
Módulo de cizallamiento | 20.0 °C | 46 GPa Show Material materials with Módulo de cizallamiento of 46 GPa |
Módulo elástico | 20.0 °C | 124 GPa Show Material materials with Módulo elástico of 124 GPa |
100.0 °C | 123 GPa Show Material materials with Módulo elástico of 123 GPa | |
200.0 °C | 118 GPa Show Material materials with Módulo elástico of 118 GPa | |
300.0 °C | 113 GPa Show Material materials with Módulo elástico of 113 GPa | |
400.0 °C | 107 GPa Show Material materials with Módulo elástico of 107 GPa | |
500.0 °C | 98 GPa Show Material materials with Módulo elástico of 98 GPa | |
600.0 °C | 88 GPa Show Material materials with Módulo elástico of 88 GPa | |
700.0 °C | 78 GPa Show Material materials with Módulo elástico of 78 GPa | |
Resistencia a la tracción | 20.0 °C | 240 - 270 MPa Show Material materials with Resistencia a la tracción of 240 - 270 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 376 - 377 J/(kg·K) Show Material materials with Calor específico of 376 - 377 J/(kg·K) | |
100.0 °C | 398 J/(kg·K) Show Material materials with Calor específico of 398 J/(kg·K) | ||
200.0 °C | 410 J/(kg·K) Show Material materials with Calor específico of 410 J/(kg·K) | ||
300.0 °C | 419 J/(kg·K) Show Material materials with Calor específico of 419 J/(kg·K) | ||
400.0 °C | 431 J/(kg·K) Show Material materials with Calor específico of 431 J/(kg·K) | ||
500.0 °C | 444 J/(kg·K) Show Material materials with Calor específico of 444 J/(kg·K) | ||
600.0 °C | 452 J/(kg·K) Show Material materials with Calor específico of 452 J/(kg·K) | ||
700.0 °C | 465 J/(kg·K) Show Material materials with Calor específico of 465 J/(kg·K) | ||
Coeficiente de dilatación térmica | 200.0 °C | 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9E-5 1/K | |
Conductividad térmica | 20.0 °C | 184 W/(m·K) Show Material materials with Conductividad térmica of 184 W/(m·K) | |
80.0 °C | 197 W/(m·K) Show Material materials with Conductividad térmica of 197 W/(m·K) | ||
120.0 °C | 209 W/(m·K) Show Material materials with Conductividad térmica of 209 W/(m·K) | ||
160.0 °C | 218 W/(m·K) Show Material materials with Conductividad térmica of 218 W/(m·K) | ||
200.0 °C | 226 W/(m·K) Show Material materials with Conductividad térmica of 226 W/(m·K) | ||
Temperatura de fusión | 875 - 1075 °C Show Material materials with Temperatura de fusión of 875 - 1075 °C | Typical for Wrought Copper Brass |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 20.0 °C | 2.47E+7 - 2.50E+7 S/m Show Material materials with Conductividad eléctrica of 2.47E+7 - 2.50E+7 S/m |
Resistividad eléctrica | 20.0 °C | 4.1E-8 Ω·m Show Material materials with Resistividad eléctrica of 4.1E-8 Ω·m |
Specific Electrical conductivity | 43 % IACS Show Material materials with Specific Electrical conductivity of 43 % IACS |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % |
Cobre | 89 - 91 % Show Material materials with Cobre of 89 - 91 % |
Estaño | 0.1 % Show Material materials with Estaño of 0.1 % |
Hierro | 0.05 % Show Material materials with Hierro of 0.05 % |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % |
Plomo | 0.05 % Show Material materials with Plomo of 0.05 % |