General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.8 - 8.9 g/cm³ Show Material materials with Densidad of 8.8 - 8.9 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | Typical for Wrought Copper Pure / Low Alloyed Copper |
Dureza Brinell | 20.0 °C | 80 - 110 [-] Show Material materials with Dureza Brinell of 80 - 110 [-] | |
Elongación | 20.0 °C | 7 - 12 % Show Material materials with Elongación of 7 - 12 % | |
Elongation A10 | 20.0 °C | 5 - 7 % Show Material materials with Elongation A10 of 5 - 7 % | |
Elongation A100 | 20.0 °C | 2 - 3 % Show Material materials with Elongation A100 of 2 - 3 % | |
Elongation A11.3 | 20.0 °C | 4 - 5 % Show Material materials with Elongation A11.3 of 4 - 5 % | |
Límite elástico Rp 0,2 | 20.0 °C | 180 - 200 MPa Show Material materials with Límite elástico Rp 0,2 of 180 - 200 MPa | |
Módulo de cizallamiento | 23.0 °C | 48 GPa Show Material materials with Módulo de cizallamiento of 48 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Módulo elástico | 20.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | |
Resistencia a la tracción | 20.0 °C | 250 - 350 MPa Show Material materials with Resistencia a la tracción of 250 - 350 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 377 - 420 J/(kg·K) Show Material materials with Calor específico of 377 - 420 J/(kg·K) | Typical for Wrought Copper Pure / Low Alloyed Copper |
Coeficiente de dilatación térmica | 300.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | |
Conductividad térmica | 20.0 °C | 368 W/(m·K) Show Material materials with Conductividad térmica of 368 W/(m·K) | |
Temperatura de fusión | 965 - 1100 °C Show Material materials with Temperatura de fusión of 965 - 1100 °C | Typical for Wrought Copper Pure / Low Alloyed Copper |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 20.0 °C | 5.00E+7 - 5.45E+7 S/m Show Material materials with Conductividad eléctrica of 5.00E+7 - 5.45E+7 S/m |
Specific Electrical conductivity | 86 % IACS Show Material materials with Specific Electrical conductivity of 86 % IACS |
Chemical properties
Property | Value |
---|---|
Fósforo | 0 - 0.01 % Show Material materials with Fósforo of 0 - 0.01 % |
Telurio | 0.4 - 0.7 % Show Material materials with Telurio of 0.4 - 0.7 % |