General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 8.9 g/cm³ Show Material materials with Densidad of 8.9 g/cm³ | Typical for Wrought Copper Pure / Low Alloyed Copper |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | Typical for Wrought Copper Pure / Low Alloyed Copper |
Límite elástico Rp0.5 | 23.0 °C | 205 MPa Show Material materials with Límite elástico Rp0.5 of 205 MPa | |
Módulo de cizallamiento | 23.0 °C | 48 GPa Show Material materials with Módulo de cizallamiento of 48 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Módulo elástico | 23.0 °C | 95 - 98 GPa Show Material materials with Módulo elástico of 95 - 98 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Resistencia a la tracción | 23.0 °C | 250 MPa Show Material materials with Resistencia a la tracción of 250 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 377 - 420 J/(kg·K) Show Material materials with Calor específico of 377 - 420 J/(kg·K) | Typical for Wrought Copper Pure / Low Alloyed Copper |
Coeficiente de dilatación térmica | 23.0 °C | 1.6E-5 - 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.8E-5 1/K | Typical for Wrought Copper Pure / Low Alloyed Copper |
Temperatura de fusión | 965 - 1100 °C Show Material materials with Temperatura de fusión of 965 - 1100 °C | Typical for Wrought Copper Pure / Low Alloyed Copper |
Chemical properties
Property | Value |
---|---|
Antimonio | 4E-4 % Show Material materials with Antimonio of 4E-4 % |
Arsénico | 5E-4 % Show Material materials with Arsénico of 5E-4 % |
Cobre | 99.99 % Show Material materials with Cobre of 99.99 % |
Cromo | 1E-4 % Show Material materials with Cromo of 1E-4 % |
Estaño | 2E-4 % Show Material materials with Estaño of 2E-4 % |
Fósforo | 3E-4 % Show Material materials with Fósforo of 3E-4 % |
Hierro | 1E-3 % Show Material materials with Hierro of 1E-3 % |
Manganeso | 5E-5 % Show Material materials with Manganeso of 5E-5 % |
Níquel | 1E-3 % Show Material materials with Níquel of 1E-3 % |
Plomo | 5E-4 % Show Material materials with Plomo of 5E-4 % |
Zinc | 1E-4 % Show Material materials with Zinc of 1E-4 % |