General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.5 - 8.55 g/cm³ Show Material materials with Densidad of 8.5 - 8.55 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | |
Dureza Brinell | 20.0 °C | 50 - 80 [-] Show Material materials with Dureza Brinell of 50 - 80 [-] | |
Dureza Vickers | 20.0 °C | 55 - 115 [-] Show Material materials with Dureza Vickers of 55 - 115 [-] | |
Elongación | 20.0 °C | 50 - 65 % Show Material materials with Elongación of 50 - 65 % | |
200.0 °C | 58 % Show Material materials with Elongación of 58 % | ||
Elongation A10 | 20.0 °C | 45 % Show Material materials with Elongation A10 of 45 % | |
Elongation A100 | 20.0 °C | 30 - 40 % Show Material materials with Elongation A100 of 30 - 40 % | |
Límite elástico Rp 0,2 | 20.0 °C | 130 - 180 MPa Show Material materials with Límite elástico Rp 0,2 of 130 - 180 MPa | |
200.0 °C | 126 MPa Show Material materials with Límite elástico Rp 0,2 of 126 MPa | ||
Módulo de cizallamiento | 23.0 °C | 40 GPa Show Material materials with Módulo de cizallamiento of 40 GPa | Typical for Wrought Copper Brass |
Módulo elástico | 20.0 °C | 114 - 115 GPa Show Material materials with Módulo elástico of 114 - 115 GPa | |
100.0 °C | 112 GPa Show Material materials with Módulo elástico of 112 GPa | ||
200.0 °C | 107 GPa Show Material materials with Módulo elástico of 107 GPa | ||
300.0 °C | 103 GPa Show Material materials with Módulo elástico of 103 GPa | ||
400.0 °C | 96 GPa Show Material materials with Módulo elástico of 96 GPa | ||
500.0 °C | 88 GPa Show Material materials with Módulo elástico of 88 GPa | ||
Resistencia a la tracción | 20.0 °C | 280 - 450 MPa Show Material materials with Resistencia a la tracción of 280 - 450 MPa | |
100.0 °C | 300 MPa Show Material materials with Resistencia a la tracción of 300 MPa | ||
150.0 °C | 295 MPa Show Material materials with Resistencia a la tracción of 295 MPa | ||
200.0 °C | 280 - 331 MPa Show Material materials with Resistencia a la tracción of 280 - 331 MPa | ||
300.0 °C | 250 MPa Show Material materials with Resistencia a la tracción of 250 MPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 377 J/(kg·K) Show Material materials with Calor específico of 377 J/(kg·K) | |
100.0 °C | 398 J/(kg·K) Show Material materials with Calor específico of 398 J/(kg·K) | ||
200.0 °C | 410 J/(kg·K) Show Material materials with Calor específico of 410 J/(kg·K) | ||
300.0 °C | 419 J/(kg·K) Show Material materials with Calor específico of 419 J/(kg·K) | ||
400.0 °C | 431 J/(kg·K) Show Material materials with Calor específico of 431 J/(kg·K) | ||
500.0 °C | 444 J/(kg·K) Show Material materials with Calor específico of 444 J/(kg·K) | ||
600.0 °C | 452 J/(kg·K) Show Material materials with Calor específico of 452 J/(kg·K) | ||
700.0 °C | 456 J/(kg·K) Show Material materials with Calor específico of 456 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100.0 °C | 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9E-5 1/K | |
150.0 °C | 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.9E-5 1/K | ||
300.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | -200.0 °C | 50 W/(m·K) Show Material materials with Conductividad térmica of 50 W/(m·K) | |
20.0 °C | 121 - 126 W/(m·K) Show Material materials with Conductividad térmica of 121 - 126 W/(m·K) | ||
200.0 °C | 147 W/(m·K) Show Material materials with Conductividad térmica of 147 W/(m·K) | ||
Temperatura de fusión | 875 - 1075 °C Show Material materials with Temperatura de fusión of 875 - 1075 °C | Typical for Wrought Copper Brass |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | -196.0 °C | 2.40E+7 S/m Show Material materials with Conductividad eléctrica of 2.40E+7 S/m |
20.0 °C | 1.60E+7 S/m Show Material materials with Conductividad eléctrica of 1.60E+7 S/m | |
200.0 °C | 1.30E+7 S/m Show Material materials with Conductividad eléctrica of 1.30E+7 S/m | |
500.0 °C | 9.00E+6 S/m Show Material materials with Conductividad eléctrica of 9.00E+6 S/m | |
Resistividad eléctrica | -196.0 °C | 4.2E-8 Ω·m Show Material materials with Resistividad eléctrica of 4.2E-8 Ω·m |
20.0 °C | 6.2E-8 Ω·m Show Material materials with Resistividad eléctrica of 6.2E-8 Ω·m | |
200.0 °C | 7.7E-8 Ω·m Show Material materials with Resistividad eléctrica of 7.7E-8 Ω·m | |
500.0 °C | 1.08E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-7 Ω·m | |
Specific Electrical conductivity | 28 % IACS Show Material materials with Specific Electrical conductivity of 28 % IACS |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % |
Cobre | 69 - 71 % Show Material materials with Cobre of 69 - 71 % |
Estaño | 0.1 % Show Material materials with Estaño of 0.1 % |
Hierro | 0.05 % Show Material materials with Hierro of 0.05 % |
Níquel | 0.3 % Show Material materials with Níquel of 0.3 % |
Plomo | 0.05 % Show Material materials with Plomo of 0.05 % |