General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8 g/cm³ Show Material materials with Densidad of 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | 23.0 °C | 40 % Show Material materials with Elongación of 40 % | |
Límite elástico | 23.0 °C | 310 MPa Show Material materials with Límite elástico of 310 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 23.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | |
Resistencia a la tracción | 23.0 °C | 680 MPa Show Material materials with Resistencia a la tracción of 680 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 23.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | |
Conductividad térmica | 23.0 °C | 14 W/(m·K) Show Material materials with Conductividad térmica of 14 W/(m·K) | |
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Resistividad eléctrica | 23.0 °C | 8.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0 - 0.03 % Show Material materials with Azufre of 0 - 0.03 % |
Carbono | 0 - 0.03 % Show Material materials with Carbono of 0 - 0.03 % |
Cromo | 16.5 - 20 % Show Material materials with Cromo of 16.5 - 20 % |
Fósforo | 0 - 0.05 % Show Material materials with Fósforo of 0 - 0.05 % |
Hierro | 54.4 - 66.9 % Show Material materials with Hierro of 54.4 - 66.9 % |
Manganeso | 0 - 2 % Show Material materials with Manganeso of 0 - 2 % |
Molibdeno | 4 - 5 % Show Material materials with Molibdeno of 4 - 5 % |
Nitrógeno | 0.1 - 0.22 % Show Material materials with Nitrógeno of 0.1 - 0.22 % |
Níquel | 12.5 - 17.5 % Show Material materials with Níquel of 12.5 - 17.5 % |