General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8.41 - 8.8 g/cm³ Show Material materials with Densidad of 8.41 - 8.8 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Rockwell B | 23.0 °C | 45 - 85 [-] Show Material materials with Dureza Rockwell B of 45 - 85 [-] |
Elongación | 23.0 °C | 17 - 60 % Show Material materials with Elongación of 17 - 60 % |
Límite elástico Rp 0,2 | 23.0 °C | 130 - 280 MPa Show Material materials with Límite elástico Rp 0,2 of 130 - 280 MPa |
Módulo elástico | 23.0 °C | 120 - 131 GPa Show Material materials with Módulo elástico of 120 - 131 GPa |
Resistencia a la tracción | 23.0 °C | 410 - 590 MPa Show Material materials with Resistencia a la tracción of 410 - 590 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 23.0 °C | 410 J/(kg·K) Show Material materials with Calor específico of 410 J/(kg·K) |
Coeficiente de dilatación térmica | 23.0 °C | 1.6E-5 - 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.75E-5 1/K |
Conductividad térmica | 23.0 °C | 105 - 110 W/(m·K) Show Material materials with Conductividad térmica of 105 - 110 W/(m·K) |
Temperatura de fusión | 870 °C Show Material materials with Temperatura de fusión of 870 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 6.2E-6 - 7.89E-6 Ω·m Show Material materials with Resistividad eléctrica of 6.2E-6 - 7.89E-6 Ω·m |
Specific Electrical conductivity | 22 - 28 % IACS Show Material materials with Specific Electrical conductivity of 22 - 28 % IACS |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminio | 0 - 0.2 % Show Material materials with Aluminio of 0 - 0.2 % | |
Berilio | 1.6 - 1.85 % Show Material materials with Berilio of 1.6 - 1.85 % | |
Cobalto | 0.2 % Show Material materials with Cobalto of 0.2 % | min. Nickel + Cobalt |
Cobre | 96.3 - 98.2 % Show Material materials with Cobre of 96.3 - 98.2 % | Balance |
Hierro | 0 - 0.6 % Show Material materials with Hierro of 0 - 0.6 % | max., Nickel + Cobalt + Iron |
Níquel | 0.2 - 0.6 % Show Material materials with Níquel of 0.2 - 0.6 % | min. Nickel + Cobalt |
Otro | 0 - 0.5 % Show Material materials with Otro of 0 - 0.5 % | |
Silicona | 0 - 0.2 % Show Material materials with Silicona of 0 - 0.2 % |
Technological properties
Property | ||
---|---|---|
Application areas | Typical applications for parts finished by forging or extrusion of these alloys include undersea instrument and repeater housings, generator rings, and resistance welding components. |