General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 2.1 g/cm³ Show Material materials with Densidad of 2.1 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Magnesium |
Elongación | 23.0 °C | 4 - 5.7 % Show Material materials with Elongación of 4 - 5.7 % | |
Límite elástico | 23.0 °C | 180 - 190 MPa Show Material materials with Límite elástico of 180 - 190 MPa | |
Módulo de cizallamiento | 23.0 °C | 45 GPa Show Material materials with Módulo de cizallamiento of 45 GPa | Typical for Magnesium |
Módulo elástico | 23.0 °C | 44 GPa Show Material materials with Módulo elástico of 44 GPa | |
Resistencia a la tracción | 23.0 °C | 280 - 300 MPa Show Material materials with Resistencia a la tracción of 280 - 300 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 23.0 °C | 960 J/(kg·K) Show Material materials with Calor específico of 960 J/(kg·K) |
Coeficiente de dilatación térmica | 23.0 °C | 2.5E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5E-5 1/K |
Conductividad térmica | 23.0 °C | 26 W/(m·K) Show Material materials with Conductividad térmica of 26 W/(m·K) |
Temperatura de fusión | 570 °C Show Material materials with Temperatura de fusión of 570 °C |
Chemical properties
Property | Value |
---|---|
Circonio | 0.4 - 1 % Show Material materials with Circonio of 0.4 - 1 % |
Cobre | 0 - 0.03 % Show Material materials with Cobre of 0 - 0.03 % |
Hierro | 0 - 0.01 % Show Material materials with Hierro of 0 - 0.01 % |
Itrio | 4.8 - 5.5 % Show Material materials with Itrio of 4.8 - 5.5 % |
Litio | 0 - 0.2 % Show Material materials with Litio of 0 - 0.2 % |
Magnesio | 88.7 - 93.4 % Show Material materials with Magnesio of 88.7 - 93.4 % |
Manganeso | 0 - 0.15 % Show Material materials with Manganeso of 0 - 0.15 % |
Níquel | 0 - 5E-3 % Show Material materials with Níquel of 0 - 5E-3 % |
Otro | 0 - 0.3 % Show Material materials with Otro of 0 - 0.3 % |
Silicona | 0 - 0.01 % Show Material materials with Silicona of 0 - 0.01 % |
Tierras raras | 1.5 - 4 % Show Material materials with Tierras raras of 1.5 - 4 % |
Zinc | 0 - 0.2 % Show Material materials with Zinc of 0 - 0.2 % |