General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 1.9 g/cm³ Show Material materials with Densidad of 1.9 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Magnesium |
Elongación | 23.0 °C | 4.1 % Show Material materials with Elongación of 4.1 % | |
Límite elástico | 23.0 °C | 130 MPa Show Material materials with Límite elástico of 130 MPa | |
Módulo de cizallamiento | 23.0 °C | 45 GPa Show Material materials with Módulo de cizallamiento of 45 GPa | Typical for Magnesium |
Módulo elástico | 23.0 °C | 48 GPa Show Material materials with Módulo elástico of 48 GPa | |
Resistencia a la tracción | 23.0 °C | 270 MPa Show Material materials with Resistencia a la tracción of 270 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 990 J/(kg·K) Show Material materials with Calor específico of 990 J/(kg·K) | |
Coeficiente de dilatación térmica | 23.0 °C | 2.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.6E-5 1/K | |
Conductividad térmica | 23.0 °C | 153 - 167 W/(m·K) Show Material materials with Conductividad térmica of 153 - 167 W/(m·K) | Typical for Magnesium |
Temperatura de fusión | 470 °C Show Material materials with Temperatura de fusión of 470 °C |
Chemical properties
Property | Value |
---|---|
Aluminio | 8.1 - 9.3 % Show Material materials with Aluminio of 8.1 - 9.3 % |
Cobre | 0 - 0.1 % Show Material materials with Cobre of 0 - 0.1 % |
Magnesio | 88.6 - 91.4 % Show Material materials with Magnesio of 88.6 - 91.4 % |
Manganeso | 0.13 - 0.35 % Show Material materials with Manganeso of 0.13 - 0.35 % |
Níquel | 0 - 0.01 % Show Material materials with Níquel of 0 - 0.01 % |
Otro | 0 - 0.3 % Show Material materials with Otro of 0 - 0.3 % |
Silicona | 0 - 0.3 % Show Material materials with Silicona of 0 - 0.3 % |
Zinc | 0.4 - 1 % Show Material materials with Zinc of 0.4 - 1 % |