DuraSense Eco PP S40 Food

Nombres alternativos y comerciales
PP-WF40
Want to keep this datasheet? Save it now in your required format

Description

Biobased Polypropylene (PP) reinforced with 40% S-Wood fiber (Biocomposite).

This grade is also available as oil-based polypropylene.

Physical properties are measured at 23°C and 50% RH

Related Standards

Los datos sobre este material han sido proporcionados por Stora Enso Biocomposites.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueComment

Bio-based content

100.0 %

Show Supplier Material materials with Bio-based content of 100.0 %

Densidad

23 °C

1.07 g/cm³

Show Supplier Material materials with Densidad of 1.07 g/cm³

ISO 1183

Mecánica

PropertyTemperatureValueComment

Elongación

23 °C

2.3 %

Show Supplier Material materials with Elongación of 2.3 %

ISO 527-2/50

Módulo de flexión

23 °C

4.4 GPa

Show Supplier Material materials with Módulo de flexión of 4.4 GPa

ISO 527-2/2

Módulo elástico

23 °C

5.2 GPa

Show Supplier Material materials with Módulo elástico of 5.2 GPa

ISO 527-2/2

Resistencia a la tracción

23 °C

45 MPa

Show Supplier Material materials with Resistencia a la tracción of 45 MPa

ISO 527-2/50

Resistencia al choque, ensayo Charpy no entallado

23 °C

15 kJ/m²

Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 15 kJ/m²

ISO 179/1eU

Aplicaciones térmicas

PropertyValue

Inflamabilidad

UL94: HB

Rheological Properties

PropertyTemperatureValueComment

Velocidad de flujo de la masa derretida

23 °C

20 g/10min

Show Supplier Material materials with Velocidad de flujo de la masa derretida of 20 g/10min

ISO 1133, 220°C/5kg

Technological properties

Property
Certifications

  • Chemical substances: REACH Compliant
  • Raw material: FSC/PEFC™ Chain of Custody
  • Food Applications: EU10/2011, GB4806.6-2016
  • Production: Approved according to GMP (Good Manufacturing Practice)
  • Toys: EN 71-3, GB 6675.1-2014
  • ISO certifications: ISO 9001/14001/50001/ OHSAS18001
  • International Sustainability and Carbon Certification: ICSS Plus
  • Fillers

    40% S-Wood Fiber

    Other

    General safety instructions, read also Process instructions:

  • Avoid high temperatures an long residence time. At high temperature fibers may degrade and can result in pressure build up in machine.
  • Avoid large piles of purged material, can start to smolder
  • Keep reject material from flammable materials, let cool before disposal i.e in water
  • Processing methods

    Drying: 2 hours at 105°C

    Injection moulding machine Temperatures:

  • Nozzle temp: 180 - 205°C
  • Zones used: 180 - 200°C
  • Zones unused: 150 - 180°C
  • Hot runner: 180 - 205°C

  • The below instructions may differ on due to injection speed, machine etc. Read process intructions.

  • Injection speed: Start slow and increase to fill the mold
  • Holding pressure: At least 50% of injection pressure
  • Holding time: Until gate freeze or lower
  • Cooling time: Approx 2 sek/mm wall thickness
  • Shot size: 25-75% of machine capacity, increase shot by approx. 10% compared to unfilled polymer