General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 7.95 g/cm³ Show Supplier Material materials with Densidad of 7.95 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Vickers | 23.0 °C | 140 - 200 [-] Show Supplier Material materials with Dureza Vickers of 140 - 200 [-] | Typical values for strip |
Elongación A50 | 20.0 °C | 37 % Show Supplier Material materials with Elongación A50 of 37 % | Typical mechanical properties for strip |
100.0 °C | 42 % Show Supplier Material materials with Elongación A50 of 42 % | Typical mechanical properties for strip | |
300.0 °C | 44 % Show Supplier Material materials with Elongación A50 of 44 % | Typical mechanical properties for strip | |
500.0 °C | 40 % Show Supplier Material materials with Elongación A50 of 40 % | Typical mechanical properties for strip | |
600.0 °C | 48 % Show Supplier Material materials with Elongación A50 of 48 % | Typical mechanical properties for strip | |
700.0 °C | 61 % Show Supplier Material materials with Elongación A50 of 61 % | Typical mechanical properties for strip | |
800.0 °C | 29 % Show Supplier Material materials with Elongación A50 of 29 % | Typical mechanical properties for strip | |
900.0 °C | 22 % Show Supplier Material materials with Elongación A50 of 22 % | Typical mechanical properties for strip | |
1000.0 °C | 23 % Show Supplier Material materials with Elongación A50 of 23 % | Typical mechanical properties for strip | |
Límite elástico Rp 0,2 | 20.0 °C | 330 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 330 MPa | Typical mechanical properties for strip |
100.0 °C | 272 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 272 MPa | Typical mechanical properties for strip | |
300.0 °C | 228 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 228 MPa | Typical mechanical properties for strip | |
500.0 °C | 203 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 203 MPa | Typical mechanical properties for strip | |
600.0 °C | 192 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 192 MPa | Typical mechanical properties for strip | |
700.0 °C | 170 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 170 MPa | Typical mechanical properties for strip | |
800.0 °C | 132 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 132 MPa | Typical mechanical properties for strip | |
900.0 °C | 74 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 74 MPa | Typical mechanical properties for strip | |
1000.0 °C | 34 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 34 MPa | Typical mechanical properties for strip | |
Resistencia a la tracción | 20.0 °C | 689 MPa Show Supplier Material materials with Resistencia a la tracción of 689 MPa | Typical mechanical properties for strip |
100.0 °C | 611 MPa Show Supplier Material materials with Resistencia a la tracción of 611 MPa | Typical mechanical properties for strip | |
300.0 °C | 595 MPa Show Supplier Material materials with Resistencia a la tracción of 595 MPa | Typical mechanical properties for strip | |
500.0 °C | 582 MPa Show Supplier Material materials with Resistencia a la tracción of 582 MPa | Typical mechanical properties for strip | |
600.0 °C | 510 MPa Show Supplier Material materials with Resistencia a la tracción of 510 MPa | Typical mechanical properties for strip | |
700.0 °C | 319 MPa Show Supplier Material materials with Resistencia a la tracción of 319 MPa | Typical mechanical properties for strip | |
800.0 °C | 156 MPa Show Supplier Material materials with Resistencia a la tracción of 156 MPa | Typical mechanical properties for strip | |
900.0 °C | 88 MPa Show Supplier Material materials with Resistencia a la tracción of 88 MPa | Typical mechanical properties for strip | |
1000.0 °C | 39 MPa Show Supplier Material materials with Resistencia a la tracción of 39 MPa | Typical mechanical properties for strip | |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 20.0 °C | 490 J/(kg·K) Show Supplier Material materials with Calor específico of 490 J/(kg·K) |
100.0 °C | 500 J/(kg·K) Show Supplier Material materials with Calor específico of 500 J/(kg·K) | |
200.0 °C | 510 J/(kg·K) Show Supplier Material materials with Calor específico of 510 J/(kg·K) | |
400.0 °C | 540 J/(kg·K) Show Supplier Material materials with Calor específico of 540 J/(kg·K) | |
600.0 °C | 595 J/(kg·K) Show Supplier Material materials with Calor específico of 595 J/(kg·K) | |
800.0 °C | 600 J/(kg·K) Show Supplier Material materials with Calor específico of 600 J/(kg·K) | |
1000.0 °C | 640 J/(kg·K) Show Supplier Material materials with Calor específico of 640 J/(kg·K) | |
Coeficiente de dilatación térmica | 200.0 °C | 1.64E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.64E-5 1/K |
400.0 °C | 1.67E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.67E-5 1/K | |
600.0 °C | 1.7E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | |
800.0 °C | 1.73E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.73E-5 1/K | |
1000.0 °C | 1.78E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.78E-5 1/K | |
Conductividad térmica | 20.0 °C | 12 W/(m·K) Show Supplier Material materials with Conductividad térmica of 12 W/(m·K) |
100.0 °C | 13 W/(m·K) Show Supplier Material materials with Conductividad térmica of 13 W/(m·K) | |
200.0 °C | 14 W/(m·K) Show Supplier Material materials with Conductividad térmica of 14 W/(m·K) | |
400.0 °C | 18 W/(m·K) Show Supplier Material materials with Conductividad térmica of 18 W/(m·K) | |
600.0 °C | 21 W/(m·K) Show Supplier Material materials with Conductividad térmica of 21 W/(m·K) | |
800.0 °C | 23 W/(m·K) Show Supplier Material materials with Conductividad térmica of 23 W/(m·K) | |
1000.0 °C | 26 W/(m·K) Show Supplier Material materials with Conductividad térmica of 26 W/(m·K) | |
Temperatura de fusión | 1350 - 1395 °C Show Supplier Material materials with Temperatura de fusión of 1350 - 1395 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.06E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.06E-6 Ω·m |
100.0 °C | 1.09E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.09E-6 Ω·m | |
200.0 °C | 1.12E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
300.0 °C | 1.16E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.16E-6 Ω·m | |
400.0 °C | 1.18E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
500.0 °C | 1.21E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.21E-6 Ω·m | |
600.0 °C | 1.22E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.22E-6 Ω·m | |
700.0 °C | 1.24E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
800.0 °C | 1.25E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.25E-6 Ω·m | |
900.0 °C | 1.27E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.27E-6 Ω·m | |
1000.0 °C | 1.28E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.28E-6 Ω·m | |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminio | 0.5 % Show Supplier Material materials with Aluminio of 0.5 % | max. | |
Azufre | 0.03 % Show Supplier Material materials with Azufre of 0.03 % | max. | |
Carbono | 0.12 % Show Supplier Material materials with Carbono of 0.12 % | max. | |
Cobre | 0.5 % Show Supplier Material materials with Cobre of 0.5 % | max. | |
Cromo | 20 - 23 % Show Supplier Material materials with Cromo of 20 - 23 % | ||
Fósforo | 0.03 % Show Supplier Material materials with Fósforo of 0.03 % | max. | |
Hierro | Balance | ||
Lantano | 0.03 - 0.2 % Show Supplier Material materials with Lantano of 0.03 - 0.2 % | ||
Manganeso | 1 % Show Supplier Material materials with Manganeso of 1 % | max. | |
Níquel | 36 - 39 % Show Supplier Material materials with Níquel of 36 - 39 % | ||
Silicona | 1.3 - 2.2 % Show Supplier Material materials with Silicona of 1.3 - 2.2 % |
Technological properties
Property | ||
---|---|---|
Application areas | Electric furnaces, open heating elements for appliances, resistors, exhaust systems. | |
Cold Forming | For cold working the solution-annealed condition is recommended. | |
Corrosion properties | Cronifer® 40 B shows excellent oxidation resistance. This is the result of its high chromium and silicon content. The scale is very resistant to spalling because of the addition of about 0.1 % lanthanum. | |
General machinability | Cronifer® 40 B can be hot and cold worked and machined. | |
Heat Treatment | Solution annealing can be performed at temperatures typically above 1150°C., followed by quenching in water or fast cooling with air or a protective atmosphere. After cold forming a recrystallization heat treatment typically above 1150°C., is required. | |
Other | Cronifer® 40 B has a face-centered-cubic structure. |