VDM® Alloy K-500

Nombres alternativos y comerciales
Nicorros Al, Monel K-500, VDM® Alloy K-500
Want to keep this datasheet? Save it now in your required format

Description

2.4375 (NiCu30Al) is a nickel-copper alloy that can be age-hardened due to additions of aluminum and titanium. It stands out for its corrosion resistance and high strength even at elevated temperatures. The alloy is non-magnetic. VDM® Alloy K-500 is available in cold or hot-formed condition or with subsequent heat treatment in solution-annealed or age-hardened condition. It is characterized by the following features and properties:


  • Excellent corrosion resistance in many applications of offshore engineering and the chemical process industry
  • Very good resistance against chloride-induced stress corrosion cracking
  • High tensile strength up to 650°C in the age hardened condition
  • Good fatigue strength in the age hardened condition
  • Non-magnetic down to -100°C
  • Equivalent Materials

    Los datos sobre este material han sido proporcionados por VDM Metals.

    A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
    Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Propiedades

    General

    PropertyTemperatureValue

    Densidad

    23.0 °C

    8.5 g/cm³

    Show Supplier Material materials with Densidad of 8.5 g/cm³

    Mecánica

    PropertyTemperatureValueComment

    Elongación

    23.0 °C

    24 %

    Show Supplier Material materials with Elongación of 24 %

    Typical mechanical properties

    Límite elástico Rp 0,2

    20.0 °C

    690 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 690 MPa

    Typical mechanical properties

    100.0 °C

    670 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 670 MPa

    Typical mechanical properties

    200.0 °C

    640 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 640 MPa

    Typical mechanical properties

    300.0 °C

    620 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 620 MPa

    Typical mechanical properties

    400.0 °C

    600 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 600 MPa

    Typical mechanical properties

    500.0 °C

    570 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 570 MPa

    Typical mechanical properties

    600.0 °C

    490 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 490 MPa

    Typical mechanical properties

    Límite elástico Rp 1,0

    20.0 °C

    1100 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 1100 MPa

    Typical mechanical properties

    100.0 °C

    1040 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 1040 MPa

    Typical mechanical properties

    200.0 °C

    1020 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 1020 MPa

    Typical mechanical properties

    300.0 °C

    980 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 980 MPa

    Typical mechanical properties

    400.0 °C

    890 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 890 MPa

    Typical mechanical properties

    500.0 °C

    750 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 750 MPa

    Typical mechanical properties

    600.0 °C

    620 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 620 MPa

    Typical mechanical properties

    Unlock all property charts

    Módulo elástico

    20.0 °C

    179 GPa

    Show Supplier Material materials with Módulo elástico of 179 GPa

    100.0 °C

    178 GPa

    Show Supplier Material materials with Módulo elástico of 178 GPa

    200.0 °C

    176 GPa

    Show Supplier Material materials with Módulo elástico of 176 GPa

    300.0 °C

    173 GPa

    Show Supplier Material materials with Módulo elástico of 173 GPa

    400.0 °C

    168 GPa

    Show Supplier Material materials with Módulo elástico of 168 GPa

    500.0 °C

    164 GPa

    Show Supplier Material materials with Módulo elástico of 164 GPa

    600.0 °C

    162 GPa

    Show Supplier Material materials with Módulo elástico of 162 GPa

    700.0 °C

    158 GPa

    Show Supplier Material materials with Módulo elástico of 158 GPa

    Unlock all property charts

    Resistencia a la tracción

    20.0 °C

    1100 MPa

    Show Supplier Material materials with Resistencia a la tracción of 1100 MPa

    100.0 °C

    1040 MPa

    Show Supplier Material materials with Resistencia a la tracción of 1040 MPa

    200.0 °C

    1020 MPa

    Show Supplier Material materials with Resistencia a la tracción of 1020 MPa

    300.0 °C

    980 MPa

    Show Supplier Material materials with Resistencia a la tracción of 980 MPa

    400.0 °C

    890 MPa

    Show Supplier Material materials with Resistencia a la tracción of 890 MPa

    500.0 °C

    750 MPa

    Show Supplier Material materials with Resistencia a la tracción of 750 MPa

    600.0 °C

    620 MPa

    Show Supplier Material materials with Resistencia a la tracción of 620 MPa

    Unlock all property charts

    Resistencia al choque, ensayo Charpy entallado

    23.0 °C

    680 kJ/m²

    Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 680 kJ/m²

    Typical mechanical properties

    Aplicaciones térmicas

    PropertyTemperatureValue

    Calor específico

    -130.0 °C

    323 J/(kg·K)

    Show Supplier Material materials with Calor específico of 323 J/(kg·K)

    20.0 °C

    420 J/(kg·K)

    Show Supplier Material materials with Calor específico of 420 J/(kg·K)

    100.0 °C

    454 J/(kg·K)

    Show Supplier Material materials with Calor específico of 454 J/(kg·K)

    200.0 °C

    480 J/(kg·K)

    Show Supplier Material materials with Calor específico of 480 J/(kg·K)

    300.0 °C

    491 J/(kg·K)

    Show Supplier Material materials with Calor específico of 491 J/(kg·K)

    400.0 °C

    500 J/(kg·K)

    Show Supplier Material materials with Calor específico of 500 J/(kg·K)

    500.0 °C

    517 J/(kg·K)

    Show Supplier Material materials with Calor específico of 517 J/(kg·K)

    600.0 °C

    538 J/(kg·K)

    Show Supplier Material materials with Calor específico of 538 J/(kg·K)

    700.0 °C

    567 J/(kg·K)

    Show Supplier Material materials with Calor específico of 567 J/(kg·K)

    800.0 °C

    613 J/(kg·K)

    Show Supplier Material materials with Calor específico of 613 J/(kg·K)

    900.0 °C

    685 J/(kg·K)

    Show Supplier Material materials with Calor específico of 685 J/(kg·K)

    Unlock all property charts

    Coeficiente de dilatación térmica

    -130.0 °C

    1.23E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.23E-5 1/K

    100.0 °C

    1.37E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.37E-5 1/K

    200.0 °C

    1.46E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.46E-5 1/K

    300.0 °C

    1.49E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K

    400.0 °C

    1.52E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.52E-5 1/K

    500.0 °C

    1.55E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.55E-5 1/K

    600.0 °C

    1.6E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K

    700.0 °C

    1.66E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.66E-5 1/K

    800.0 °C

    1.7E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K

    900.0 °C

    1.75E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.75E-5 1/K

    Unlock all property charts

    Conductividad térmica

    -130.0 °C

    13.3 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 13.3 W/(m·K)

    20.0 °C

    17.4 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 17.4 W/(m·K)

    100.0 °C

    19.4 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 19.4 W/(m·K)

    200.0 °C

    20.9 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 20.9 W/(m·K)

    300.0 °C

    25.1 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 25.1 W/(m·K)

    400.0 °C

    27.8 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 27.8 W/(m·K)

    500.0 °C

    30.5 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 30.5 W/(m·K)

    600.0 °C

    33.1 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 33.1 W/(m·K)

    700.0 °C

    35.7 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 35.7 W/(m·K)

    800.0 °C

    37.4 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 37.4 W/(m·K)

    900.0 °C

    41.2 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 41.2 W/(m·K)

    Unlock all property charts

    Eléctrico

    PropertyTemperatureValue

    Resistividad eléctrica

    20.0 °C

    6.1E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.1E-7 Ω·m

    100.0 °C

    6.2E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.2E-7 Ω·m

    200.0 °C

    6.3E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.3E-7 Ω·m

    300.0 °C

    6.5E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.5E-7 Ω·m

    400.0 °C

    6.5E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.5E-7 Ω·m

    500.0 °C

    6.5E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.5E-7 Ω·m

    600.0 °C

    6.6E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.6E-7 Ω·m

    700.0 °C

    6.6E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.6E-7 Ω·m

    800.0 °C

    6.7E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.7E-7 Ω·m

    900.0 °C

    6.8E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 6.8E-7 Ω·m

    Unlock all property charts

    Magnético

    PropertyTemperatureValueComment

    Permeabilidad magnética relativa

    23.0 °C

    1 [-]

    Show Supplier Material materials with Permeabilidad magnética relativa of 1 [-]

    max.

    Temperatura de Curie

    -135 °C

    Show Supplier Material materials with Temperatura de Curie of -135 °C

    Typical material property in solution annealed condition, Solution annealed and age hardened: -100°C

    Chemical properties

    PropertyValueComment

    Aluminio

    2.3 - 3.15 %

    Show Supplier Material materials with Aluminio of 2.3 - 3.15 %

    Azufre

    0.01 %

    Show Supplier Material materials with Azufre of 0.01 %

    max.

    Carbono

    0.18 %

    Show Supplier Material materials with Carbono of 0.18 %

    max.

    Cobre

    27 - 33 %

    Show Supplier Material materials with Cobre of 27 - 33 %

    Estaño

    6E-3 %

    Show Supplier Material materials with Estaño of 6E-3 %

    max.

    Fósforo

    0.02 %

    Show Supplier Material materials with Fósforo of 0.02 %

    max.

    Hierro

    0.5 - 2 %

    Show Supplier Material materials with Hierro of 0.5 - 2 %

    Manganeso

    1.5 %

    Show Supplier Material materials with Manganeso of 1.5 %

    max.

    Níquel

    63 %

    Show Supplier Material materials with Níquel of 63 %

    min.

    Plomo

    6E-3 %

    Show Supplier Material materials with Plomo of 6E-3 %

    max.

    Silicona

    0.5 %

    Show Supplier Material materials with Silicona of 0.5 %

    max.

    Titanio

    0.35 - 0.85 %

    Show Supplier Material materials with Titanio of 0.35 - 0.85 %

    Zinc

    0.02 %

    Show Supplier Material materials with Zinc of 0.02 %

    max.

    Technological properties

    Property
    Application areas

    VDM® Alloy K-500 is used in sea water, offshore engineering, in the chemical process and petrochemicals industry and shipbuilding. Typical applications are: Valve seals, pump sleeves and wearing rings in sea water, pump shafts and propeller shafts, mounting elements and fasteners, e.g. bolts in sea air and splash water zones, tug rope armoring, springs, components of drilling equipment in the oil industry, aircraft instrument components.

    Cold Forming

    Cold forming should be conducted on annealed material. VDM® Alloy K-500 has similar forming and strain hardening properties as austenitic stainless steels. This must be taken into account during design and selection of forming tools and equipment and during the planning of forming processes. To achieve a high strength, a combination of cold forming with subsequent age hardening is an option.

    Corrosion properties

    The corrosion resistance of VDM® Alloy K-500 is generally equivalent to that of VDM® Alloy 400. The alloy proves excellent resistance against many media, from pure water to highly concentrated salt solutions and alkalis. VDM® Alloy K-500 is virtually immune against stress corrosion cracking induced by chloric ions. In the age hardened condition, the material can be sensitive to stress corrosion cracking in hot hydrofluoric acid vapor under tensions near the yield strength. In fast-flowing seawater and in sea air, good resistance is proven but in hardly moving or standing sea water, pitting can occur. VDM® Alloy K-500 is also very resistant against acid gas media.

    General machinability

    VDM® Alloy K-500 is preferably processed in the annealed condition. The best results in terms of the surface quality of the finished product are achieved, however, by pre-treatment before age hardening and finishing after age hardening. Age hardened material can undergo a heat treatment for the purpose of tension compensation after the finishing. Since the alloy has a tendency to strain hardening, a low cutting speed should be selected and the cutting tool should stay engaged at all times. An adequate chip depth is important in order to cut below a previously formed strain-hardened zone. Optimum heat dissipation through the use of large quantities of suitable, preferably aqueous, lubricants has con-siderable influence on a stable machining process.

    Heat Treatment

    Annealing is conducted in the temperature range from 850 to 1,000°C (1,562 to 1,832°F) with retention times between 3 and 5 minutes per mm thickness and preferably in 980°C (1,796°F). Temperatures above 1,000°C (1,832°F) are not recommendable because strong grain growth can occur. Cooling down in water or accelerated cooling down in the air with thicknesses of less than 3 mm (0.12 in) or diameters of less than 12.5 mm (0.49 in) is recommendable and important so to avoid precipitations. The tension compensation achieved by retention times of 1 to 2 hours at 300 to 350°C (572 to 662°F) with subsequent cooling down in the air is necessary to remove the tension concentration from material that has been machined before the age hardening. The tension compensation is also recommendable for material that contains tensions from the cold forming after the last heat treatment, e.g. for straightening.

    Hot forming

    VDM® K-500 can be hot-formed in a temperature range from 900 to 1,150°C (1,652 to 2,102°F) with subsequent rapid cooling down in water. Cooling down in the air can cause age hardening and then lead to cracks when the material is heated up again. After the hot forming, annealing between 850 and 900°C (1,562 and 1,652°F) with subsequent water quenching is recommendable for compensating tensions and any mixed microstructure. The subsequent deformation should be at least 25 % and be implemented below 1,050°C (1,922°F) to achieve an optimal toughness.

    Other

    VDM® Alloy K-500 has a face-centered cubic lattice. In the age hardened condition, the γ’ phase is precipitated.

    Welding

    The material can be welded using all conventional methods: GTAW (TIG), GTAW (TIG) hot wire, plasma, MIG and submerged arc welding. The material should be in its solution-annealed condition for welding, and should be free of scale, grease and markings. Application of the impulse technique is preferable in gas-shielded metal welding processes. When welding the root, care should be taken to achieve best quality root protection using pure argon (argon 4.6), so that the welding edge is free from oxides after welding the root. Root protection is also recommended for the first and, in certain cases depending on the welded construction, also for the second intermediate layer weld after root welding. Any heat tint must be removed, preferably using a stainless steel brush, while the welding edge is still hot. The interpass temperature should be max. 120°C (248°F). After the welding and before the age hardening, it is recommended to anneal the components between 850°C and 900°C (1,562 to 1,652°F) with subsequent cooling down as quickly as possible.