General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 4.505 g/cm³ Show Material materials with Densidad of 4.505 g/cm³ | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.361 [-] Show Material materials with Coeficiente de Poisson of 0.361 [-] | Typical for Pure Titanium | ||||
Dureza Brinell | 20.0 °C | 120.0 Show Material materials with Dureza Brinell of 120.0 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | |
20.0 °C | 120.0 Show Material materials with Dureza Brinell of 120.0 | Annealed | DIN 17864, DIN 17851, DIN 17862, DIN 17860 | Forging | Transverse | |
Elongación | 20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Welded Tube | ||
Estricción | 20.0 °C | 35.0 % Show Material materials with Estricción of 35.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 35.0 % Show Material materials with Estricción of 35.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Módulo de cizallamiento | 20.0 °C | 45.0 GPa Show Material materials with Módulo de cizallamiento of 45.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Sheet, Strip, Welded Tube | |
Módulo elástico | 20.0 °C | 108.0 GPa Show Material materials with Módulo elástico of 108.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | |
200.0 °C | 95.0 GPa Show Material materials with Módulo elástico of 95.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | ||
400.0 °C | 82.0 GPa Show Material materials with Módulo elástico of 82.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | ||
Resistencia a la tracción | 20.0 °C | 290.0 - 410.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 410.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Welded Tube | |
20.0 °C | 290.0 - 410.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 410.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse | |
20.0 °C | 350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
100.0 °C | 280.0 MPa Show Material materials with Resistencia a la tracción of 280.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
200.0 °C | 175.0 MPa Show Material materials with Resistencia a la tracción of 175.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
300.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 520.0 J/(kg·K) Show Material materials with Calor específico of 520.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Calor específico of 570.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Calor específico of 630.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | ||
Coeficiente de dilatación térmica | 200.0 °C | 8.7e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 8.7e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Sheet, Strip, Welded Tube | |
400.0 °C | 8.5e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 8.5e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Sheet, Strip, Welded Tube | ||
Conductividad térmica | 20.0 °C | 22.6 W/(m·K) Show Material materials with Conductividad térmica of 22.6 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | |
200.0 °C | 20.9 W/(m·K) Show Material materials with Conductividad térmica of 20.9 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | ||
400.0 °C | 19.3 W/(m·K) Show Material materials with Conductividad térmica of 19.3 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | ||
Temperatura de fusión | 1670.0 °C Show Material materials with Temperatura de fusión of 1670.0 °C | Typical for Pure Titanium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Resistividad eléctrica | 20.0 °C | 4.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
200.0 °C | 8.2e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.2e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube | |
400.0 °C | 1.18e-06 Ω·m Show Material materials with Resistividad eléctrica of 1.18e-06 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbono | 0.06 Show Material materials with Carbono of 0.06 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Hidrógeno | 0.013 Show Material materials with Hidrógeno of 0.013 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Hierro | 0.15 Show Material materials with Hierro of 0.15 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Nitrógeno | 0.05 Show Material materials with Nitrógeno of 0.05 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Oxígeno | 0.12 Show Material materials with Oxígeno of 0.12 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Paladio | 0.15 - 0.25 % Show Material materials with Paladio of 0.15 - 0.25 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Sheet, Strip, Welded Tube |
Titanio | 99.0 % Show Material materials with Titanio of 99.0 % | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tube, Rod, Forging, Sheet, Strip, Welded Tube |