General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 6.51 g/cm³ Show Material materials with Densidad of 6.51 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.35 [-] Show Material materials with Coeficiente de Poisson of 0.35 [-] |
Módulo de cizallamiento | 20.0 °C | 36.2 GPa Show Material materials with Módulo de cizallamiento of 36.2 GPa |
Módulo elástico | 20.0 °C | 99.2 GPa Show Material materials with Módulo elástico of 99.2 GPa |
38.0 °C | 98.6 GPa Show Material materials with Módulo elástico of 98.6 GPa | |
93.0 °C | 93.1 GPa Show Material materials with Módulo elástico of 93.1 GPa | |
149.0 °C | 86.9 GPa Show Material materials with Módulo elástico of 86.9 GPa | |
204.0 °C | 80.7 GPa Show Material materials with Módulo elástico of 80.7 GPa | |
260.0 °C | 75.2 GPa Show Material materials with Módulo elástico of 75.2 GPa | |
316.0 °C | 69.6 GPa Show Material materials with Módulo elástico of 69.6 GPa | |
371.0 °C | 64.1 GPa Show Material materials with Módulo elástico of 64.1 GPa | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 100.0 °C | 284.7 J/(kg·K) Show Material materials with Calor específico of 284.7 J/(kg·K) | |
Coeficiente de dilatación térmica | 23.0 °C | 5.7E-6 - 7E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 5.7E-6 - 7E-6 1/K | Typical for Zirconium |
Conductividad térmica | 20.0 °C | 22 W/(m·K) Show Material materials with Conductividad térmica of 22 W/(m·K) | |
Temperatura de fusión | 1845 °C Show Material materials with Temperatura de fusión of 1845 °C | Typical for Zirconium |
Chemical properties
Property | Value |
---|---|
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Hafmio | 4.5 % Show Material materials with Hafmio of 4.5 % |
Hidrógeno | 4E-3 % Show Material materials with Hidrógeno of 4E-3 % |
Nitrógeno | 0.02 % Show Material materials with Nitrógeno of 0.02 % |
Oxígeno | 0.16 % Show Material materials with Oxígeno of 0.16 % |