General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 4.505 g/cm³ Show Material materials with Densidad of 4.505 g/cm³ | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.361 [-] Show Material materials with Coeficiente de Poisson of 0.361 [-] | Typical for Pure Titanium | ||||
Módulo de cizallamiento | 46.0 GPa Show Material materials with Módulo de cizallamiento of 46.0 GPa | Typical for Pure Titanium | ||||
Módulo elástico | 20.0 °C | 108.0 GPa Show Material materials with Módulo elástico of 108.0 GPa | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | |
200.0 °C | 95.0 GPa Show Material materials with Módulo elástico of 95.0 GPa | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | ||
400.0 °C | 81.0 GPa Show Material materials with Módulo elástico of 81.0 GPa | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 540.0 J/(kg·K) Show Material materials with Calor específico of 540.0 J/(kg·K) | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Calor específico of 570.0 J/(kg·K) | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Calor específico of 630.0 J/(kg·K) | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | ||
Coeficiente de dilatación térmica | 8.400000000000001e-06 - 8.599999999999999e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 8.400000000000001e-06 - 8.599999999999999e-06 1/K | Typical for Pure Titanium | ||||
Conductividad térmica | 20.0 °C | 20.1 W/(m·K) Show Material materials with Conductividad térmica of 20.1 W/(m·K) | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | |
200.0 °C | 20.1 W/(m·K) Show Material materials with Conductividad térmica of 20.1 W/(m·K) | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | ||
400.0 °C | 20.5 W/(m·K) Show Material materials with Conductividad térmica of 20.5 W/(m·K) | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | ||
Temperatura de fusión | 1670.0 °C Show Material materials with Temperatura de fusión of 1670.0 °C | Typical for Pure Titanium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Resistividad eléctrica | 20.0 °C | 5.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.5e-07 Ω·m | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
200.0 °C | 8.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.8e-07 Ω·m | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat | |
400.0 °C | 1.22e-06 Ω·m Show Material materials with Resistividad eléctrica of 1.22e-06 Ω·m | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbono | 0.06 Show Material materials with Carbono of 0.06 | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Hidrógeno | 0.013 Show Material materials with Hidrógeno of 0.013 | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Hierro | 0.3 Show Material materials with Hierro of 0.3 | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Nitrógeno | 0.05 Show Material materials with Nitrógeno of 0.05 | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Oxígeno | 0.35 Show Material materials with Oxígeno of 0.35 | Welded | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Flat |
Titanio | 98.8 % Show Material materials with Titanio of 98.8 % | Welded | WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860 | Flat |