General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 5 g/cm³ Show Material materials with Densidad of 5 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Zinc Aluminium |
Dureza Brinell | 20.0 °C | 110 - 120 [-] Show Material materials with Dureza Brinell of 110 - 120 [-] | |
Elongación A50 | 20.0 °C | 3 - 6 % Show Material materials with Elongación A50 of 3 - 6 % | |
Límite elástico Rp 0,2 | 20.0 °C | 338 - 345 MPa Show Material materials with Límite elástico Rp 0,2 of 338 - 345 MPa | |
Módulo elástico | 20.0 °C | 75 GPa Show Material materials with Módulo elástico of 75 GPa | |
Resistencia a la tracción | 20.0 °C | 400 - 440 MPa Show Material materials with Resistencia a la tracción of 400 - 440 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 393 - 525 J/(kg·K) Show Material materials with Calor específico of 393 - 525 J/(kg·K) | Typical for Zinc Aluminium |
Coeficiente de dilatación térmica | 23.0 °C | 2.2E-5 - 2.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2E-5 - 2.8E-5 1/K | Typical for Zinc Aluminium |
Conductividad térmica | 23.0 °C | 105 - 125 W/(m·K) Show Material materials with Conductividad térmica of 105 - 125 W/(m·K) | Typical for Zinc Aluminium |
Temperatura de fusión | 375 - 485 °C Show Material materials with Temperatura de fusión of 375 - 485 °C | Typical for Zinc Aluminium |
Chemical properties
Property | Value |
---|---|
Aluminio | 25 - 28 % Show Material materials with Aluminio of 25 - 28 % |
Cadmio | 3E-3 % Show Material materials with Cadmio of 3E-3 % |
Cobre | 2 - 2.5 % Show Material materials with Cobre of 2 - 2.5 % |
Estaño | 2E-3 % Show Material materials with Estaño of 2E-3 % |
Hierro | 0.1 % Show Material materials with Hierro of 0.1 % |
Magnesio | 0.01 - 0.02 % Show Material materials with Magnesio of 0.01 - 0.02 % |
Plomo | 4E-3 % Show Material materials with Plomo of 4E-3 % |
Zinc | 69.37 % Show Material materials with Zinc of 69.37 % |
Technological properties
Property | ||
---|---|---|
Processing methods | sand casting |