General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 10.5 g/cm³ Show Material materials with Densidad of 10.5 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.37 [-] Show Material materials with Coeficiente de Poisson of 0.37 [-] | Typical for Silver |
Dureza Vickers | 20.0 °C | 70 [-] Show Material materials with Dureza Vickers of 70 [-] | |
Módulo de cizallamiento | 20.0 °C | 26 GPa Show Material materials with Módulo de cizallamiento of 26 GPa | |
Módulo elástico | -195.0 °C | 89 GPa Show Material materials with Módulo elástico of 89 GPa | |
20.0 °C | 80 GPa Show Material materials with Módulo elástico of 80 GPa | ||
200.0 °C | 77 GPa Show Material materials with Módulo elástico of 77 GPa | ||
400.0 °C | 67 GPa Show Material materials with Módulo elástico of 67 GPa | ||
600.0 °C | 57 GPa Show Material materials with Módulo elástico of 57 GPa | ||
800.0 °C | 46 GPa Show Material materials with Módulo elástico of 46 GPa | ||
900.0 °C | 40 GPa Show Material materials with Módulo elástico of 40 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 234 - 251 J/(kg·K) Show Material materials with Calor específico of 234 - 251 J/(kg·K) | Typical for Silver |
Coeficiente de dilatación térmica | 100.0 °C | 1.79E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.79E-5 1/K | |
150.0 °C | 1.86E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.86E-5 1/K | ||
200.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
250.0 °C | 1.92E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.92E-5 1/K | ||
300.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
350.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
400.0 °C | 1.99E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.99E-5 1/K | ||
450.0 °C | 2.01E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.01E-5 1/K | ||
500.0 °C | 2.04E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.04E-5 1/K | ||
600.0 °C | 2.12E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.12E-5 1/K | ||
700.0 °C | 2.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.25E-5 1/K | ||
800.0 °C | 2.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36E-5 1/K | ||
900.0 °C | 2.43E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.43E-5 1/K | ||
Conductividad térmica | -233.0 °C | 1050 W/(m·K) Show Material materials with Conductividad térmica of 1050 W/(m·K) | |
-173.0 °C | 475 W/(m·K) Show Material materials with Conductividad térmica of 475 W/(m·K) | ||
-73.0 °C | 441 W/(m·K) Show Material materials with Conductividad térmica of 441 W/(m·K) | ||
20.0 °C | 419 W/(m·K) Show Material materials with Conductividad térmica of 419 W/(m·K) | ||
127.0 °C | 426 W/(m·K) Show Material materials with Conductividad térmica of 426 W/(m·K) | ||
327.0 °C | 411 W/(m·K) Show Material materials with Conductividad térmica of 411 W/(m·K) | ||
527.0 °C | 397 W/(m·K) Show Material materials with Conductividad térmica of 397 W/(m·K) | ||
927.0 °C | 383 W/(m·K) Show Material materials with Conductividad térmica of 383 W/(m·K) | ||
Temperatura de fusión | 962 °C Show Material materials with Temperatura de fusión of 962 °C | Typical for Silver |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 20.0 °C | 6.00E+7 S/m Show Material materials with Conductividad eléctrica of 6.00E+7 S/m |
Resistividad eléctrica | 20.0 °C | 1.67E-8 - 1.8E-8 Ω·m Show Material materials with Resistividad eléctrica of 1.67E-8 - 1.8E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Plata | 99.97 % Show Material materials with Plata of 99.97 % |