General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 10.2 g/cm³ Show Material materials with Densidad of 10.2 g/cm³ | Typical for Molybdenum |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Molybdenum |
Elongación A50 | 20.0 °C | 1 - 18 % Show Material materials with Elongación A50 of 1 - 18 % | |
Límite elástico | 20.0 °C | 550 - 655 MPa Show Material materials with Límite elástico of 550 - 655 MPa | |
Módulo de cizallamiento | 23.0 °C | 125 GPa Show Material materials with Módulo de cizallamiento of 125 GPa | Typical for Molybdenum |
Módulo elástico | 23.0 °C | 324 GPa Show Material materials with Módulo elástico of 324 GPa | Typical for Molybdenum |
Resistencia a la tracción | 20.0 °C | 655 - 795 MPa Show Material materials with Resistencia a la tracción of 655 - 795 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 201 - 280 J/(kg·K) Show Material materials with Calor específico of 201 - 280 J/(kg·K) | Typical for Molybdenum |
Coeficiente de dilatación térmica | 23.0 °C | 4E-6 - 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 4E-6 - 1.4E-5 1/K | Typical for Molybdenum |
Conductividad térmica | 23.0 °C | 117 - 431 W/(m·K) Show Material materials with Conductividad térmica of 117 - 431 W/(m·K) | Typical for Molybdenum |
Temperatura de fusión | 2610 °C Show Material materials with Temperatura de fusión of 2610 °C | Typical for Molybdenum |
Chemical properties
Property | Value |
---|---|
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Hierro | 0.01 % Show Material materials with Hierro of 0.01 % |
Nitrógeno | 2E-3 % Show Material materials with Nitrógeno of 2E-3 % |
Níquel | 2E-3 % Show Material materials with Níquel of 2E-3 % |
Oxígeno | 1.5E-3 % Show Material materials with Oxígeno of 1.5E-3 % |
Silicona | 0.01 % Show Material materials with Silicona of 0.01 % |