Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 25 [-] Show Material materials with Dureza Brinell of 25 [-] |
50.0 °C | 20 [-] Show Material materials with Dureza Brinell of 20 [-] | |
120.0 °C | 12 [-] Show Material materials with Dureza Brinell of 12 [-] | |
150.0 °C | 8 [-] Show Material materials with Dureza Brinell of 8 [-] | |
Límite elástico Rp 0,2 | 20.0 °C | 61 MPa Show Material materials with Límite elástico Rp 0,2 of 61 MPa |
50.0 °C | 60 MPa Show Material materials with Límite elástico Rp 0,2 of 60 MPa | |
100.0 °C | 36 MPa Show Material materials with Límite elástico Rp 0,2 of 36 MPa | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Conductividad térmica | 23.0 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | Typical for Tin Antimony |
Temperatura de fusión | 215 - 350 °C Show Material materials with Temperatura de fusión of 215 - 350 °C | Typical for Tin Antimony |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.01 % Show Material materials with Aluminio of 0.01 % |
Antimonio | 11 - 13 % Show Material materials with Antimonio of 11 - 13 % |
Arsénico | 0.1 % Show Material materials with Arsénico of 0.1 % |
Bismuto | 0.08 % Show Material materials with Bismuto of 0.08 % |
Cobre | 5 - 7 % Show Material materials with Cobre of 5 - 7 % |
Hierro | 0.1 % Show Material materials with Hierro of 0.1 % |
Plomo | 1 - 3 % Show Material materials with Plomo of 1 - 3 % |
Zinc | 0.01 % Show Material materials with Zinc of 0.01 % |