Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 22 [-] Show Material materials with Dureza Brinell of 22 [-] |
50.0 °C | 17 [-] Show Material materials with Dureza Brinell of 17 [-] | |
100.0 °C | 10 [-] Show Material materials with Dureza Brinell of 10 [-] | |
120.0 °C | 11 [-] Show Material materials with Dureza Brinell of 11 [-] | |
150.0 °C | 8 [-] Show Material materials with Dureza Brinell of 8 [-] | |
Límite elástico Rp 0,2 | 20.0 °C | 46 - 47 MPa Show Material materials with Límite elástico Rp 0,2 of 46 - 47 MPa |
50.0 °C | 44 MPa Show Material materials with Límite elástico Rp 0,2 of 44 MPa | |
100.0 °C | 27 MPa Show Material materials with Límite elástico Rp 0,2 of 27 MPa | |
Resistencia a la tracción | 20.0 °C | 77 MPa Show Material materials with Resistencia a la tracción of 77 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Conductividad térmica | 23.0 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | Typical for Tin Antimony |
Temperatura de fusión | 215 - 350 °C Show Material materials with Temperatura de fusión of 215 - 350 °C | Typical for Tin Antimony |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.01 % Show Material materials with Aluminio of 0.01 % |
Antimonio | 7 - 8 % Show Material materials with Antimonio of 7 - 8 % |
Arsénico | 0.1 % Show Material materials with Arsénico of 0.1 % |
Bismuto | 0.08 % Show Material materials with Bismuto of 0.08 % |
Cadmio | 0.05 % Show Material materials with Cadmio of 0.05 % |
Cobre | 3 - 4 % Show Material materials with Cobre of 3 - 4 % |
Hierro | 0.1 % Show Material materials with Hierro of 0.1 % |
Plomo | 0.35 % Show Material materials with Plomo of 0.35 % |
Zinc | 0.01 % Show Material materials with Zinc of 0.01 % |