Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.77 g/cm³ Show Supplier Material materials with Density of 1.77 g/cm³ | dry | ISO 1183 | |
Limiting oxygen index | 37 % Show Supplier Material materials with Limiting oxygen index of 37 % | dry | ISO 4589-1/-2 | |
Moisture absorption | 1.4 % Show Supplier Material materials with Moisture absorption of 1.4 % | dry | Sim. to ISO 62 | |
Water absorption | 1.45 % Show Supplier Material materials with Water absorption of 1.45 % | dry | ISO 62 | at 23°C after 24h |
5.1 % Show Supplier Material materials with Water absorption of 5.1 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 10 GPa Show Supplier Material materials with Elastic modulus of 10 GPa | conditioned | ISO 527-1/-2 | |||
10.5 GPa Show Supplier Material materials with Elastic modulus of 10.5 GPa | conditioned | ISO 527-1/-2 | ||||
15 GPa Show Supplier Material materials with Elastic modulus of 15 GPa | dry | ISO 527-1/-2 | ||||
15 GPa Show Supplier Material materials with Elastic modulus of 15 GPa | dry | ISO 527-1/-2 | 1 mm | |||
120 °C | 9.5 GPa Show Supplier Material materials with Elastic modulus of 9.5 GPa | dry | ISO 527-1/-2 | |||
160 °C | 6.5 GPa Show Supplier Material materials with Elastic modulus of 6.5 GPa | dry | ISO 527-1/-2 | |||
Elongation | 1.8 % Show Supplier Material materials with Elongation of 1.8 % | dry | ISO 527-1/-2 | |||
1.8 % Show Supplier Material materials with Elongation of 1.8 % | dry | ISO 527-1/-2 | 1 mm | |||
3 % Show Supplier Material materials with Elongation of 3 % | conditioned | ISO 527-1/-2 | ||||
3 % Show Supplier Material materials with Elongation of 3 % | conditioned | ISO 527-1/-2 | ||||
120 °C | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |||
160 °C | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |||
Flexural modulus | 10 GPa Show Supplier Material materials with Flexural modulus of 10 GPa | conditioned | ISO 178 | |||
13.5 GPa Show Supplier Material materials with Flexural modulus of 13.5 GPa | dry | ISO 178 | ||||
120 °C | 8.5 GPa Show Supplier Material materials with Flexural modulus of 8.5 GPa | dry | ISO 178 | |||
160 °C | 5.5 GPa Show Supplier Material materials with Flexural modulus of 5.5 GPa | dry | ISO 178 | |||
Flexural yield strength | 240 MPa Show Supplier Material materials with Flexural yield strength of 240 MPa | conditioned | ISO 178 | |||
300 MPa Show Supplier Material materials with Flexural yield strength of 300 MPa | dry | ISO 178 | ||||
120 °C | 190 MPa Show Supplier Material materials with Flexural yield strength of 190 MPa | dry | ISO 178 | |||
160 °C | 130 MPa Show Supplier Material materials with Flexural yield strength of 130 MPa | dry | ISO 178 | |||
Impact strength, Charpy notched | -30 °C | 14.0 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 14.0 kJ/m² | dry, conditioned | ISO 179/1eA | ||
23 °C | 13 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m² | dry | ISO 179/1eA | |||
23 °C | 14.0 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 14.0 kJ/m² | conditioned | ISO 179/1eA | |||
Impact strength, Charpy unnotched | -30 °C | 40 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m² | dry, conditioned | ISO 179/1eU | ||
23 °C | 50 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 50 kJ/m² | dry | ISO 179/1eU | |||
23 °C | 70 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 70 kJ/m² | conditioned | ISO 179/1eU | |||
Tensile strength | 130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | conditioned | ISO 527-1/-2 | |||
130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | conditioned | ISO 527-1/-2 | at low thickness | |||
190 MPa Show Supplier Material materials with Tensile strength of 190 MPa | dry | ISO 527-1/-2 | ||||
200 MPa Show Supplier Material materials with Tensile strength of 200 MPa | dry | ISO 527-1/-2 | 1 mm | at low thickness | ||
120 °C | 100 MPa Show Supplier Material materials with Tensile strength of 100 MPa | dry | ISO 527-1/-2 | |||
160 °C | 85 MPa Show Supplier Material materials with Tensile strength of 85 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Ball pressure temperature | 275 °C Show Supplier Material materials with Ball pressure temperature of 275 °C | dry | IEC 60695-10-2 | |||
Coefficient of thermal expansion | 1.7e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.7e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 6.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.75 mm | |||
Glow Wire Ignition Temperature | 850 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 850 °C | dry | IEC 60695-2-13 | 0.75 mm | ||
960 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 960 °C | dry | IEC 60695-2-13 | 3 mm | |||
Heat deflection temperature | 290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | dry | UL746B | 0.35 mm | ||
Relative temperature index, mechanical impact | 110 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 110 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 120 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 120 °C | dry | UL746B | 0.75 mm | ||
Thermal diffusivity | 1.4e-07 mm²/s Show Supplier Material materials with Thermal diffusivity of 1.4e-07 mm²/s | dry | - | |||
Vicat softening temperature | 290 °C Show Supplier Material materials with Vicat softening temperature of 290 °C | dry | ISO 306 | 50°C/h 50N |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 325 V Show Supplier Material materials with Comparative tracking index of 325 V | dry | IEC 60112 | |
Dielectric constant | 3.6 [-] Show Supplier Material materials with Dielectric constant of 3.6 [-] | dry | IEC 60250 | 1GHz |
3.8 [-] Show Supplier Material materials with Dielectric constant of 3.8 [-] | conditioned | IEC 60250 | 1GHz | |
4 [-] Show Supplier Material materials with Dielectric constant of 4 [-] | dry | IEC 62631-2-1 | 1MHz | |
4.3 [-] Show Supplier Material materials with Dielectric constant of 4.3 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.5 [-] Show Supplier Material materials with Dielectric constant of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
12 [-] Show Supplier Material materials with Dielectric constant of 12 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 20 kV/mm Show Supplier Material materials with Dielectric strength of 20 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Dielectric strength of 30 kV/mm | dry | IEC 60243-1 | ||
Dissipation factor | 60 [-] Show Supplier Material materials with Dissipation factor of 60 [-] | dry | IEC 62631-2-1 | 100Hz |
160 [-] Show Supplier Material materials with Dissipation factor of 160 [-] | dry | IEC 62631-2-1 | 1MHz | |
250 [-] Show Supplier Material materials with Dissipation factor of 250 [-] | dry | IEC 60250 | 1GHz | |
325 [-] Show Supplier Material materials with Dissipation factor of 325 [-] | conditioned | IEC 60250 | 1GHz | |
700 [-] Show Supplier Material materials with Dissipation factor of 700 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3300 [-] Show Supplier Material materials with Dissipation factor of 3300 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+08 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+08 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1570 g/cm³ Show Supplier Material materials with Density of melt of 1570 g/cm³ | dry | - | |
Shrinkage | 0.3 % Show Supplier Material materials with Shrinkage of 0.3 % | dry | Sim. to ISO 294-4 | Parallel |
0.9 % Show Supplier Material materials with Shrinkage of 0.9 % | dry | Sim. to ISO 294-4 | Normal | |
Specific heat capacity melt | 1550 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1550 J/(kg·K) | dry | - | |
Spiral flow length | 200 | dry | - | 1.0 mm 800 bar |
215 | dry | - | 1.0 mm 900 bar | |
230 | dry | - | 1.0 mm 1000 bar | |
95 | dry | - | 0.5mm 1200 bar | |
115 | dry | - | 0.5mm 1600 bar | |
135 | dry | - | 0.5mm 2000 bar | |
Thermal conductivity of melt | 0.335 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.335 W/(m·K) | dry | - | |
Viscosity number | 80 cm³/gr Show Supplier Material materials with Viscosity number of 80 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | FPC connectors, WtB and BtB Connectors, Battery Connectors | |
Certifications | Yellow Card Available | |
Fillers | 40% Glass Fiber |