Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.76 g/cm³ Show Material materials with Dichte of 2.76 g/cm³ | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 69.0 - 72.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 72.0 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Härte, Brinell | 125.0 [-] Show Material materials with Härte, Brinell of 125.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 125.0 [-] Show Material materials with Härte, Brinell of 125.0 [-] | T651 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Schubmodule | 26.4 - 27.1 GPa Show Material materials with Schubmodule of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Zugfestigkeit | 390.0 MPa Show Material materials with Zugfestigkeit of 390.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
400.0 MPa Show Material materials with Zugfestigkeit of 400.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
410.0 MPa Show Material materials with Zugfestigkeit of 410.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 390.0 MPa Show Material materials with Zugfestigkeit of 390.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 400.0 MPa Show Material materials with Zugfestigkeit of 400.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 410.0 MPa Show Material materials with Zugfestigkeit of 410.0 MPa | T651 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.1e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 - 2.4e-05 1/K | Typical for Wrought 7000 Series Aluminium |
Schmelzpunkt | 465.0 - 655.0 °C Show Material materials with Schmelzpunkt of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Spezifische Wärmekapazität | 795.0 - 1050.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium |
Wärmeleitfähigkeit | 121.0 - 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121.0 - 170.0 W/(m·K) | Typical for Wrought 7000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.2 % Show Material materials with Chrom of 0.2 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Eisen | 0.45 % Show Material materials with Eisen of 0.45 % | T651 | EN 573-3 | Flat |
0.45 % Show Material materials with Eisen of 0.45 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Magnesium | 1.5 - 2.5 % Show Material materials with Magnesium of 1.5 - 2.5 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Mangan | 0.15 - 0.5 % Show Material materials with Mangan of 0.15 - 0.5 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Nickel | 0.1 % Show Material materials with Nickel of 0.1 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Zink | 3.5 - 4.5 % Show Material materials with Zink of 3.5 - 4.5 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Zirkonium | 0.1 - 0.25 % Show Material materials with Zirkonium of 0.1 - 0.25 % | T651 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |