Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | H18 | EN 573-3, EN 485 | A50 | ||
2.0 % Show Material materials with Dehnung of 2.0 % | H18 | EN 573-3, EN 485, EN 754 | A50 | |||
2.0 % Show Material materials with Dehnung of 2.0 % | H18 | EN 573-3, EN 754 | A100 | |||
3.0 % Show Material materials with Dehnung of 3.0 % | H18 | EN 573-3, EN 1301 | ||||
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube | A10 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube | ||
Härte, Brinell | 79.0 [-] Show Material materials with Härte, Brinell of 79.0 [-] | H18 | EN 573-3, EN 485 | |||
20.0 °C | 65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube | ||
Zugfestigkeit | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | H18 | EN 573-3, EN 754 | |||
255.0 MPa Show Material materials with Zugfestigkeit of 255.0 MPa | H18 | EN 573-3, EN 485 | ||||
265.0 MPa Show Material materials with Zugfestigkeit of 265.0 MPa | H18 | EN 573-3, EN 1301 | ||||
20.0 °C | 235.0 MPa Show Material materials with Zugfestigkeit of 235.0 MPa | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 255.0 MPa Show Material materials with Zugfestigkeit of 255.0 MPa | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 610.0 - 650.0 °C Show Material materials with Schmelzpunkt of 610.0 - 650.0 °C | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
Spezifische Wärmekapazität | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 921.0 J/(kg·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube | |
Wärmeleitfähigkeit | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | H18 | EN 573-3, EN 1301, EN 485, EN 754 | |||
20.0 °C | 167.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 167.0 W/(m·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 25000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 25000000.0 - 30000000.0 S/m | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
20.0 °C | 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 26000000.0 S/m | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube | |
spezifischer Widerstand | 3.33e-08 - 4e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.33e-08 - 4e-08 Ω·m | H18 | EN 573-3, EN 1301, EN 485, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.15 % Show Material materials with Chrom of 0.15 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Flat, Tube |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Flat, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | H18 | EN 573-3, EN 1301, EN 485, EN 754 | ||
Kupfer | 0.15 % Show Material materials with Kupfer of 0.15 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Flat, Tube |
Magnesium | 1.7 - 2.4 % Show Material materials with Magnesium of 1.7 - 2.4 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Flat, Tube |
Mangan | 0.1 - 0.5 % Show Material materials with Mangan of 0.1 - 0.5 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Flat, Tube |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Flat, Tube |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Flat, Tube |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 754 | Rod, Flat, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): sufficient / poor, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12) |